Polyols as Phase Change Materials for Low-grade Excess Heat Storage

Polyols as Phase Change Materials for Low-grade Excess Heat Storage

Available online at www.sciencedirect.com ScienceDirect Energy Procedia 61 (2014) 664 – 669 The 6th International Conference on Applied Energy – ICA...

876KB Sizes 0 Downloads 18 Views

Available online at www.sciencedirect.com

ScienceDirect Energy Procedia 61 (2014) 664 – 669

The 6th International Conference on Applied Energy – ICAE2014

Polyols as phase change materials for low-grade excess heat storage

Saman Nimali Gunasekaraa*, Ruijun Pana, Justin Ningwei Chiua, and Viktoria Martina a

Energy Technology- HPT, Royal Institute of Technology (KTH), Brinellvägen 68, 100 44 Stockholm, Sweden.

Abstract Polyols are an emerging phase change materials (PCM) category for thermal energy storage (TES), with moderate phase change temperatures and considerable enthalpies. These can be employed in systems for harvesting surplus energy from, industrial and power generation processes. However, knowledge on the properties of polyols in relation to desirable PCM properties is presently sparse and rather inconsistent. This work summarizes a literature review on polyols as PCM for TES. In addition, preliminary T-History characterization of some selected polyols was done. This study is expected to be an initiation of an extensive polyol phase equilibrium evaluation. © 2014 The Gunasekara Authors. Published Ltd.NW. ThisJ., is an access under by theElsevier CC BY-NC-ND © 2014 S.N., by PanElsevier R., Chiu andopen Martin V.article Published Ltd. license (http://creativecommons.org/licenses/by-nc-nd/3.0/). Selection and/or peer-review under responsibility of ICAE Peer-review under responsibility of the Organizing Committee of ICAE2014 Keywords: Phase change materials (PCM); Polyols; T-history method; Material properties

Nomenclature °C Degrees Celsius kJ/kg Kilojoule per kilogram PCM Phase change material PEG Polyethylene Glycol TES Thermal energy storage T-History Temperature History W/(m∙K) Watt per meter, kelvin 1. Introduction One important task for reaching a sustainable energy system is to realize resource efficiency. In this context, the utilization of surplus heat from industrial processes, including large scale power generation is important. This is done internally within a plant through process integration. To a smaller extent, the heat is utilized externally by e.g. connection to a district heating system [1], [2], [3]. However, the full potential of converting excess heat into a resource cannot be realized due to the mismatch in time, and location, between source and demand. Thermal energy storage using phase change materials (PCMs) is one effective solution to explore for managing this mismatch, now emerging with considerable momentum [4], [5], e.g., for, district heating [6] and heat exchange within industries [7]. In this work, polyols (poly alcohols/sugar alcohols) are evaluated as one particular material category of PCM interest, owing to their moderate phase change temperatures of around 0-200 °C [8] and higher mass-specific and volume-specific enthalpies than other organic PCMs [8]. Furthermore, many polyols are non-toxic [9] and safe

* Corresponding author. Tel.: Office: +46 (0)8 7907476, Mobile: +46 (0)736523339; E-mail address: [email protected].

1876-6102 © 2014 The Authors. Published by Elsevier Ltd. This is an open access article under the CC BY-NC-ND license (http://creativecommons.org/licenses/by-nc-nd/3.0/). Peer-review under responsibility of the Organizing Committee of ICAE2014 doi:10.1016/j.egypro.2014.11.938

665

Saman Nimali Gunasekara et al. / Energy Procedia 61 (2014) 664 – 669

[10], [11], some even being common sugar substitutes; e.g. Erythritol, Xylitol, Lactitol [11]. Their material compatibility is similar to paraffins [9], hence compatible with metals. In pure grades, polyols are comparatively expensive. Nevertheless, being produced via carbohydrates hydrogenation [8], [11], [12], they have a potential for large-scale production, which could be expected to reduce their prices. The overall objective of this paper is to present polyols in light of the desired material behavior needed in making use of these, pure and as blends as PCMs for storage of low grade excess heat in industrial applications. Literature findings and preliminary thermal characterizations of some selected polyols are used as input for the analysis. 2. Polyols as phase change materials for thermal energy storage PCMs including polyols, have great potential in many TES applications e.g., solar [13], buildings [14], vehicles [9], and more [15], [16]. A growing PCM interest in polyols is evident at present e.g., patents on pure and blends of polyols [17] and polyol-salt blends [10] as PCM TES, plus literature on evaluation of mixtures/composites: Mannitol-fatty acid esters [18], Erythritol-porous materials [19], [20] and Polyethylene glycol-sugar [21]. However, the TES design data for polyol PCM still have gaps to be bridged, including for polyol blends. Table 1 compiles some thermal properties of pure polyols of PCM interest, from literature. Evidently many of these polyols properties, are in ranges, some inconsistent and, some with gaps particularly on thermal conductivity and fusion enthalpy. Table 1. Thermal properties of some polyols of PCM interest for TES, as found in literature Polyol Glycerol (Glycerin) CH2OH.CHOH.CH2OH (C3H8O3) Erythritol C4H6(OH)4, (C4H10O4) Teritol

D-Threitol (C4H10O4) HOCH2[CH(OH)]2 L-Threitol CH2OH [33], [34] D,L- Threitol 1-3 Butylene Glycol (1,3-Butanediol, C4H10O2) Diethylene glycol (C4H10O3) Ribitol (C5H12O5) Xylitol C5H7 (OH)5, (C5H12O5)

Arabinitol (arabitol) (C5H12O5) [33] D-Arabitol L-Arabitol Pentaerythritol (Tetramethylo1methane) (C5H12O4) Allitol Dulcitol Sorbitol (D-Sorbitol, D-Glucitol) C6H8 (OH)6 L-Glucitol D,L- Glucitol D-Mannitol C6H8 (OH)6

(C6H14O6) [33], [34]

L- Mannitol D,L- Mannitol D-Talitol L-Talitol D,L-Talitol D-Iditol L-Iditol Catechol (1,2-benzenediol) (C6H6O2) Trimethylopropane (TMP, 2,2-Dihydroxymethyl1-1Butanol) C2H5C(CH2OH)3 (C6H14O3) Triethylene glycol(C6H14O4) Galactitol C6H8 (OH)6 (Dulcitol) (C6H14O6) Heptitol

Freezin g Temp. (˚C) ~18

Glycero-gulo-heptitol D-glycero-D-ido-heptitol (C7H16O7) Perseitol Volemitol Octitol D-Erythro-D-galacto-octitol (C8H18O8) Thymol (2-Isopropyl-5-méthylphénol,C10H14O [34]

Heat of, fusion/* melting (kJ/kg)

Thermal conductivity (W/(m·K))

References

~199 315-344 ~315/~340/~355 339/332-340 ~340

~0.14/ 0.28 (at 25°C) ~0.73(S),0.33 (L) ~0.73(S,20°C), ~0.33 (L,140°C) ~0.73(S,20°C), ~0.33 (L,140°C)

[9], [22], [23], [24], [25] [9] [26], [27], [20], [16], [28] [29]/ [30] [8], [22], [31], [32], [13] [22] [22] [22] [22] [14], [23] [30]/ [22]/ [35] [22]

10 -10/-10 to -7 100/ 102/ 104 61 – 61.5** ~93/ 93.5 ~93-94.5

247 250/ /247 232±1/ ~246 232–263/258-270/ ~263/ ~240 263, 221/~237 ~219 230 ~256

94/ 94-95.5 ~96/ 95-97

Penitol

Hexitol

Melting Temp. (˚C) (**: metastable) ~18 117-118 ~118 118-121/119 120 88.5 - 90 88.5 - 90 69 -70

90 101/ 103 102 -103 185-245 186-187 155 189 93/~90-92** 95–~98/ 95±1.2 96-101 97/~(97–98)/ ~98 ~(97-99) 89-91 135 - 137 ~(163-165)/ ~(164-166) 165-168 ~166/ 166-168 ~167 162 - 163 168 88 -89 87 -88 95-96 73.5 ~(76-77) ~104 57 - 59 -7 167-185 188/ 188-189 129 129 187 153 169-170 51.5

287-298

110-185/ 165±1 196-217 185 ~171/~166

~270/~273

117

294-341 ~335/ ~316 316, *~261

207 59 247 350-413 351/ ~352

115

[28], [35] [9], [13], [30], [31], [36] [8], [37]/ [36] [37], [38] [30] [35]/ [22] [22] [22] [30] [22] [22] [22] [9]/ [28] [30] [8], [13], [22], [31] [36] [22] [22] [36] [9] [18], [22]/ [13] [8], [13], [39] [22] [22] [22] [22] [22] [22] [22] [31], [40] [22] [14], [23] [30] [8]/ [9], [13] [22] [22] [22] [22] [22] [40]

666

Saman Nimali Gunasekara et al. / Energy Procedia 61 (2014) 664 – 669

1-Decanol CH3(CH2)9OH (C10H22O) 1-Dodecanol (C12H26O) Maltitol (C12H24O11) Lactitol monohydrate (C12H24O11.H2O) Lactitol (C12H24O11) Palatinitol (C12H24O11 [33]) 1-Tetradecanol (C14H30O) Cetyl alcohol CH3(CH2)15OH, (C16H34O) 400 600

Polyethylene Glycol (PEG)

800 1000 1450 3000 4000 4500 6000 10000

11/ 6 26 17.5-~23 145-152 94-105 146-152 145 38 ~49 8 17-22 20-25 22/~23 28.5 ~33/35-40 52-56 ~58 55-60/ ~58/ 66 55-60/~61

205/ 206 200 ~189 173

~14 ~30/~38 45 ~36 ~56 /49.5

135–149 170 205 141 ~100 127 146 ~127 *~137 *~173/154

*~187 190/ ~180/ 176 /*~187/181

~0.19 (L, at ~39°C, 70°C) ~0.19 (L, at ~39°C, ~67°C ) ~0.19 (L, at ~39°C, ~67°C ) ~0.19 (L, at ~39°C, ~67°C )

[41]/ [9] [14], [16], [31] [31], [42] [9], [30], [32] [30] [9], [30], [32] [30] [16] [40] [14], [16], [31] [8], [14], [31] [14], [40] [14], [16], [43], [44]/ [22] [45] [45]/ [8], [22], [21] [22] [8] [45] [22] [8], [16]/ [44]/ [21] [8]/ [45]/ [21]

In addition to melting, freezing enthalpies (in kJ/kg) were available in literature for D-Mannitol: ~214 [39] and for PEG types 800, 1000, 4000 and 10000 of around: 130, 154, 152 and 142 [45] respectively. 1,2,4-Butanetriol (C4H10O4) is said to supercool [22], but with no temperature/ enthalpy indications. A comprehensive phase change understanding of polyols also is crucial in TES systems design using polyols PCM. Many polyols undergo some subcooling [8], [9], exhibit 10-15% volume expansion during melting [9], and decompose under excessive temperatures [46], [10]. For subcooling, some mitigation measures were reported; e.g. [47], [48]. Interestingly, phase transition with subcooling (with irreversible recalescence) could be less irreversible than a stable equilibrium, if the thermal conductivity ratio of solid and liquid phases is sufficiently below unity [49]. This is expected only with Biot numbers of intermediate values [49], and suggests better thermal cyclability. Many polyols are amorphous when anhydrous; undergoing glass transition. But they are plasticized by water, then becoming crystalline and thus solidify [50] (e.g. amorphous Xylitol and Sorbitol [28]). Glass transition is a state change, undesirable for a PCM because the expected sharp phase change is replaced by a continuous cooling over a wide temperature range. Glass transition temperature of polyols reduces with increasing water content and molecular weight [28]. Carbohydrates with high ratios of melting to glass transition temperature readily crystallize and have high enthalpy of fusion [28], which should also be true for polyols, for being carbohydrates. For most of these complex phase and state transitions of polyols, except for a few generalizations, comprehensive knowledge on pure components and blends of PCM TES design interest is not that available in open literature. Further, to study polyol blends, they should first-of-all be miscible in one another. Polyols are soluble in polar solvents and insoluble in non-polar solvents [51] although much details are unavailable on polyolpolyol solubility. 3. Preliminary T-history characterization of selected polyols Preliminary T-History characterization similar to [52] was done for selected polyols. The temperature histories of 99% pure Erythritol, Xylitol and synthesis grade PEG 10,000 were obtained, using two identical polyol samples and a reference (thermal Si oil) in horizontally placed glass test-tubes inside stone-wool insulated boxes, thermally cycled in an ACS Hygross 1200 climate chamber. Thermal sensors were of T-type thermocouples. Erythritol, Xylitol and PEG 10,000 exhibited considerable subcooling, probable glass transition after the first melting, and very little subcooling, respectively. These are briefly discussed with temperature histories in the Appendix for, Erythritol: Figure 1, Xylitol: Figure 2, Figure 3, and PEG: Figure 4, Figure 5, respectively. Glass transition was deduced due to an apparent smooth cooling curve replacing the expected phase change plateau, and a transparent liquid getting thicker with cooling, and ultimately becoming a rigid, transparent, glass-like material at the end of the cooling. This is not merely subcooling, judging by the appearance and thickness increase of the material, and the extended cooling range. 4. Discussion Various phase and state change behaviors like subcooling and glass transition differ even among pure polyols. For instance, Erythritol is often not reported with, and was not exhibiting glass transition, while Xylitol exhibits probable glass transition. Glass transition could possibly be related with the high hygroscopicity of Xylitol, whereas Erythritol is not hygroscopic. In contrast, PEG 10,000 exhibits proper phase change, and has negligible subcooling. Comparison of the chemical structure of PEG 10,000 to the others’ may provide a better understanding on these differences. 5. Concluding Remarks

Saman Nimali Gunasekara et al. / Energy Procedia 61 (2014) 664 – 669

The literature survey shows that there are gaps, and even some inconsistencies on thermo-physical property data of polyols as PCM for TES design. Preliminary T-History based characterization of some selected polyols has been conducted in this work. A detailed analysis of polyols on subcooling, glass transition and like behaviors also is crucial to evaluate their suitability as PCM. To consider polyol blends as PCM, miscibility of polyols should be evaluated, followed by thermal property characterization and phase equilibrium evaluation of these blends. 6. Acknowledgements The authors extend their gratitude to the Swedish Energy Agency for funding this project. 7. References [1]

A. Kapil, I. Bulatov, R. Smith and J.-K. Kim, "Process integration of low grade heat in process industry with district heating networks," Energy, vol. 44, no. 2012, pp. 11-19, 2012.

[2]

D. Connolly, H. Lund, B. V. Mathiesen, S. Werner, B. Möller, U. Persson, T. Boermans, D. Trier, P. A. Østergaard and S. Nielsen, "Heat Roadmap Europe: Combining district heating with heat savings to decarbonise the EU energy system," Energy Policy, no. Article in press, 2013.

[3]

H. Fang, J. Xia, K. Zhu, Y. Su and Y. Jiang, "Industrial waste heat utilization for low temperature district heating," Energy Policy, vol. 62, no. 2013, p. 236–246, 2013.

[4]

A. Hauer, S. Gschwander, Y. Kato, V. Martin, P. Schossig and F. Setterwall, "Transportation of Energy by Utilization of Thermal Energy Storage Technology," ECES- IEA Annex 18, 2010.

[5]

SAMSSA, "Sugar Alcohol based Material for Seasonal Storage Applications," European Community's 7th Framework Programme , 2013. [Online]. Available: http://samssa.eu/. [Accessed 09 December 2013].

[6]

H. Li , W. Wang, J. Yan and E. Dahlquist, "Economic assessment of the mobilized thermal energy storage (M-TES) system for distributed heat supply," Applied Energy, vol. 104, no. 2013, p. 178–186, 2013.

[7]

T. Nomura, N. Okinaka and T. Akiyama, "Waste heat transportation system, using phase change material (PCM) from steelworks to chemical plant," Resources, Conservation & Recycling, vol. 54, no. 2010, p. 1000–1006, 2010.

[8]

H. Mehling and L. F. Cabeza, Heat and cold storage with PCM- An up to date introduction into basics and applications, Verlag, Berlin: Springer, 2008.

[9]

N. R. Jankowski and P. F. McCluskey, "A review of phase change materials for vehicle component thermal buffering," Applied Energy, vol. 113, no. 2014, pp. 1525-1561, 2014.

[10] H. Kakiuchi, S. Chihara, M. Yamazaki and T. Isaki, "Heat Storage Material Composition". Japan/Inashiki-gun Patent 5,785,885, 28 July 1998. [11] International Food Information Council Foundation, "Sugar Alcohols Fact Sheet," 15 October 2009. [Online]. Available: http://www.foodinsight.org/Resources/Detail.aspx?topic=Sugar_Alcohols_Fact_Sheet. [Accessed 08 December 2013]. [12] Z.-X. Wang, J. Zhuge, H. Fang and B. A. Prior, "Glycerol production by microbial fermentation: A review," Biotechnology Advances, vol. 19, no. 2001, p. 201–223, 2001. [13] M. Kenisarin and K. Mahkamov, "Solar energy storage using phase change materials," Renewable and Sustainable Energy Reviews, vol. 11, no. 2007, p. 1913–1965, 2007. [14] L. F. Cabeza, A. Castell, C. Barreneche, A. d. Gracia and A. I. Fernández, "Materials used as PCM in thermal energy storage in buildings: A review," Renewable and Sustainable Energy Reviews, vol. 15, no. 2011, p. 1675– 1695, 2011. [15] E. Oró, A. d. Gracia, A. Castell, M. M. Farid and L. F. Cabeza, "Review on phase change materials (PCMs) for cold thermal energy storage applications," Applied Energy, vol. 99, no. 2012, p. 513–533, 2012. [16] B. Zalba, J. M. Marín, L. F. Cabeza and H. Mehling, "Review on thermal energy storage with phase change: materials, heat transfer analysis & applications," Applied Thermal Engineering, vol. 23, no. 2003, p. 251–283, 2003. [17] H. Gerd, "Latent heat storage material and use thereof". United States Patent 4,795,580, 3 January 1989. [18] A. Sari, "Thermal energy storage properties of mannitol–fatty acid esters as novel organic soild-liquid phase change materials," Energy Conversion and Management, vol. 64, no. 2012, pp. 68-78, 2012. [19] T. Nomura , N. Okinaka and T. Akiyama, "Impregnation of porous material with phase change material for thermal energy storage," Materials Chemistry and Physics, vol. 115, no. 2009, p. 846–850, 2009. [20] T. Oya, T. Nomura, N. Okinaka and T. Akiyama, "Phase change composite based on porous nickel and erythritol," Applied Thermal Engineering, vol. 40, no. 2012, pp. 373-377, 2012. [21] C. Alkan, E. Gunther, S. Hiebler, Ö. F. Ensari and D. Kahraman, "Polyethylene Glycol-Sugar Composites as Shape Stabilized Phase Change Materials for Thermal Energy Storage," POLYMER COMPOSITES, pp. 17281736, 2012. [22] E. W. Flick, Industrial Solvents Handbook, 5th ed., William Andrew Publishing/Noyes, 1998. [23] E. Oró, A. d. Gracia , A. Castell, M. Farid and L. F. Cabeza, "Review on phase change materials (PCMs) for cold thermal energy storage applications," Applied Energy, vol. 99, no. 2012, pp. 513-533, 2012. [24] sbioinformatics.com, "www.sbioinformatics.com," [Online]. Available: http://www.sbioinformatics.com/design_thesis/Glycerol/Glycerol_-2520Properties&uses.pdf. [Accessed 18 November 2013]. [25] J. P. Ellenberger, Piping and Pipeline Calculations Manual : Construction, Design, Fabrication and Examination, Burlington/Oxford: Elsevier Inc (Butterworth-Heinemann), 2010. [26] F. Agyenim, P. Eames and M. Smyth, "A comparison of heat transfer enhancement in a medium temperature thermal energy storage heat exchanger using fins," Solar Energy, vol. 83, no. 2009, p. 1509–1520, 2009. [27] T. Nomura, M. Tsubota, A. Sagara, N. Okinaka and T. Akiyama, "Performance analysis of heat storage of direct-contact heat exchanger with phase-change material," Applied Thermal Engineering, vol. 58, no. 2013, pp. 108-113, 2013. [28] R. A. Talja and Y. H. Roos, "Phase and state transition effects on dieelectric, mechanical and thermal properties of polyols," Thermochimica Acta, vol. 380, no. 2001, pp. 109-121, 2001. [29] A. Hesaraki, "CFD modeling of heat charging process in a direct-contact container for mobilized thermal energy storage," Mälardalen University, Sweden, Mälardalen, 2011. [30] J. Waschull, R. Müller and S. Römer, "Investigation of Phase Change Materials for Elevated Temperatures," in EffStock 2009, Stockholm, 2009. [31] A. A. Al-Abidi, S. B. Mat, K. Sopian, M. Y. Sulaiman, C. H. Lim and A. Th, "Review ofthermalenergystorageforairconditioningsystems," RenewableandSustainableEnergyReviews, vol. 16, no. 2012, p. 5802–5819, 2012. [32] D. Haillot, T. Bauer, U. Kröner and R. Tamme, "Thermal analysis of phase change materials in the temperature range 120–150 ◦C," Thermochimica Acta, vol. 513, no. 2011, pp. 49-59, 2011. [33] Sigma-Aldrich, "www.sigmaaldrich.com," Sigma-Aldrich Co. LLC., 2013. [Online]. Available: http://www.sigmaaldrich.com/catalog/product/aldrich/377619?lang=en®ion=SE. [Accessed 25 December 2013]. [34] ChemSpider, "www.chemspider.com," Royal Society of Chemistry, 2013. [Online]. Available: http://www.chemspider.com/Chemical-Structure.81747.html. [Accessed 25 December 2013]. [35] C. L. Yaws, "Yaws' Critical Property Data for Chemical Engineers and Chemists," Knovel, 2012. [36] P. Perkkalainen, H. Halttunen and I. Pitkänen, "Solid state co-crystallization of sugar alcohols measured with differential scanning calorimetry," Therrnochimica Acta, vol. 269/270, no. 1995, pp. 351-359, 1995. [37] B. Tong, Z.-C. Tan, Q. Shi, Y.-S. Li, D.-T. Yue and S.-X. Wang, "Thermodynamic investigation of several natural polyols (I): Heat capacities and thermodynamic properties of xylitol," Thermochimica Acta, vol. 457, no. 2007, p. 20–26, 2007. [38] The Royal Society of Chemistry, The Dictionary of Substances and their Effects, 3rd Electronic ed., S. Gangolli, Ed., Cambridge: The Royal Society of Chemistry, 2005. [39] E. Oró, A. Gil, L. Miró, G. Peiró, S. Álvarez and L. F. Cabeza, "Thermal energy storage implementation using phase change materials for solar cooling and refrigeration applications," Energy Procedia, vol. 30, no. 2012, p. 947 – 956, 2012. [40] A. Sharma, V. V. Tyagi, C. R. Chen and D. Buddhi, "Review on thermal energy storage with phase change materials and applications," Renewable and Sustainable Energy Reviews, vol. 13, no. 2009, pp. 318-345, 2009. [41] G. A. Lane, Solar Heat Storage: Latent Heat Material, Volume I, Florida: CRC Press Inc., 1983. [42] A. M. Khudhair and M. M. Farid, "A review on energy conservation in building applications with thermal storage by latent heat using phase change materials," Energy Conversion and Management, vol. 45, no. 2004, p. 263–275, 2004. [43] D. Zhou, C. Y. Zhao and Y. Tian, "Review on thermal energy storage with phase change materials (PCMs) in building applications," Applied Energy, vol. 92, no. 2012, p. 593–605, 2012. [44] M. M. Farid, A. M. Khudhair, S. A. K. Razack and S. Al-Hallaj, "A review on phase change energy storage: materials and applications," Energy Conversion and Management, vol. 45, no. 2004, p. 1597–1615, 2004. [45] W. Wang, "Mobilized Thermal Energy Storage for Heat Recovery for Distributed Heating," Mälardalen University, Västerås, Sweden, 2010. [46] K. Akihide , N. Maruoka, A. Kawai, H. Kamano, T. Jozuka, T. Senda and T. Akiyama, "Thermophysical and heat transfer properties of phase change material candidate for waste heat transportation system," Heat and Mass Transfer, vol. 44, no. 7, pp. 763-769, 2008. [47] N. R. Jankowski and P. F. McCluskey, "Electrical Supercooling Mitigation in Erythritol," in 2010 14th International Heat Transfer Conference, Washington, DC, 2010. [48] E. P. Ona, X. Zhang, K. Kyaw , F. Watanabe, H. Matsuda, H. Kakiuchi, M. Yabe and S. Chihara, "Relaxation of Supercooling of Erythritol for Latent Heat Storage," Journal of Chemical Engineering of Japan, vol. 34, no. No. 3, pp. 376-382, 2001. [49] A. Seppälä, "Irreversibility of solidification and of a cyclic solidification and melting process," International Journal of Heat and Mass Transfer, vol. 55, no. 2012, p. 1582–1595, 2012. [50] H. Levine and L. Slade, "Water as a plasticizer: physico-chemical aspects of low-moisture polymeric systems," in Water Science Reviews 3 - Water Dynamics, F. Franks, Ed., Cambridge, Cambridge University Press, 1988, pp. 79-185. [51] A. Harlin, "Biogenic Precursors for Polyphenol, Polyester and Polyurethane Resins," in Handbook of Bioplastics and Biocomposites Engineering Applications , Massachusetts, Scrivener Publishing LLC/John Wiley & Sons, Inc, 2011, pp. 511-553. [52] J. N. Chiu and V. Martin, "Submerged finned heat exchanger latent heat storage design and its experimental verification," Applied Energy, vol. 93, no. 2012, p. 507–516, 2012.

667

668

Saman Nimali Gunasekara et al. / Energy Procedia 61 (2014) 664 – 669

8.

Biography

All the authors are from Energy Technology (EGI), KTH- Royal Institute of Technology. S. N. Gunasekara is a PhD candidate, with M.Sc. Sustainable Technology. R. Pan is a Research Engineer, with M.Sc. Sustainable Energy Engineering. Dr. J. NW. Chiu is a Research Associate. Dr. V. Martin is an Associate Professor. 9.

Appendix T-History, Pure Erythritol

140

Temperature, (°C)

130 120 110 104,28 100

S1

90

S2 84,42

80 70 60 900

1100

1300

1500

Time (minutes)

Figure 1. Temperature-History for pure Erythritol: exhibiting subcooling during freezing. (S1 and S2 are two samples of Erythritol subjected to same conditions). Here a subcooling of around 20 °C was observed.

T-History, pure Xylitol, first heating cycle

Temperature (°C)

120 100 91,0261

80

93,3726

60

S1

40

S2

20 0 0

400

800

1200

1600

Time (min) Figure 2. Temperature-History of pure Xylitol: first heating cycle where phase change (melting) is observed around between 91-93 °C, which are rather similar in range to the literature-based expected melting temperatures. (S1 and S2 are two samples of Xylitol subjected to same conditions) Figure 3 shows the temperature-history of pure Xylitol, heating and cooling cycles after the first heating/cooling cycle. During cooling, the material appeared as a transparent glass like material, with increasing viscosity (less flowability) with decreasing temperature, which was rigid when below around -10 °C. These characteristics are attributed as probable glass-transition. Also, this behavior is deduced to be glass-transition and not subcooling due to these changes such like the increase in thickness (less flowability), and the rigid, transparent glassy nature of the material at the end of each cooling. Once this glass transition was observed, there were no further identifiable phase change plateaus even during heating cycles.

Saman Nimali Gunasekara et al. / Energy Procedia 61 (2014) 664 – 669

T-History pure Xylitol, after the first heating and melting cycle 120

Temperature (°C)

100 80 60

S1

40

S2

20 0 0

1000

2000

3000

Time (Minutes) Figure 3. Temperature-History of pure Xylitol, heating and cooling cycles after the first heating/cooling cycle where no phase change occurs within the temperature range of 120 to ~2 °C. (S1 and S2 are two samples of Xylitol subjected to same conditions)

Temperature (°C)

T-History, pure PEG 10,000: heating 80 75 70 65 60 55 50 45 40 35 30 25 20 1750

67,90 60,35

S1 S2

1950

2150

2350

Time (Min) Figure 4. Temperature- History of pure PEG 10,000 during heating. (S1 and S2 are two samples of PEG 10,000 subjected to same conditions). Exhibits melting at a temperature range of around 60-68 °C, a value rather close to the expected literature-based melting temperatures.

Temperature (°C)

T-History, pure PEG 10,000: cooling 80 75 70 65 60 55 50 45 40 35 30 25 20 2600

S1 S2

2800

3000

3200

Time (Min) Figure 5 Temperature-History of pure PEG 10,000, for cooling. Freezing occurs with only very little subcooling (of around 3 °C, circled in red), around the expected melting temperature.

669