Controlled synthesis, characterization and application of hydrophobic calcium carbonate nanoparticles in PVC

Controlled synthesis, characterization and application of hydrophobic calcium carbonate nanoparticles in PVC

    Controlled synthesis, characterization and application of hydrophobic calcium carbonate nanoparticles in PVC Lina Zhao, Yaodan Zhang,...

597KB Sizes 0 Downloads 53 Views

    Controlled synthesis, characterization and application of hydrophobic calcium carbonate nanoparticles in PVC Lina Zhao, Yaodan Zhang, Yang Miao, Lijun Nie PII: DOI: Reference:

S0032-5910(15)30144-3 doi: 10.1016/j.powtec.2015.11.001 PTEC 11322

To appear in:

Powder Technology

Received date: Revised date: Accepted date:

21 October 2014 30 October 2015 1 November 2015

Please cite this article as: Lina Zhao, Yaodan Zhang, Yang Miao, Lijun Nie, Controlled synthesis, characterization and application of hydrophobic calcium carbonate nanoparticles in PVC, Powder Technology (2015), doi: 10.1016/j.powtec.2015.11.001

This is a PDF file of an unedited manuscript that has been accepted for publication. As a service to our customers we are providing this early version of the manuscript. The manuscript will undergo copyediting, typesetting, and review of the resulting proof before it is published in its final form. Please note that during the production process errors may be discovered which could affect the content, and all legal disclaimers that apply to the journal pertain.

ACCEPTED MANUSCRIPT Controlled synthesis, characterization and

nanoparticles in PVC Yang Miao1, 2

Lijun Nie1, 2

IP

Lina Zhao1, 2 Yaodan Zhang1, 2

T

application of hydrophobic calcium carbonate

SC R

(1. College of Chemistry, Jilin Normal University, Siping 136000, China; 2. Key Laboratory of Preparation and Applications of Environmental Friendly Materials, Jilin Normal University, Ministry of Education, Siping 136000, China)

NU

Abstract: Modification of calcium carbonate particles with surfactant significantly

MA

improves the properties of polyvinyl chloride (PVC). Hydrophobic spherical CaCO3 particles were prepared in the presence of dodecyl dihydrogen phosphate (DDP) by a

D

carbonation method. In the process, DDP was used as an organic substrate to induce

TE

the nucleation and growth of calcium carbonate. The operating parameters such as

CE P

temperature and the dosage of the organic substrate were varied to study their influences on the active ratio and contact angle of calcium carbonate particles. The

AC

surface property of CaCO3 particles was changed from hydrophilic to hydrophobic when the dosage of DDP to CaCO3 changed from 0 to 2 %. The contact angle of modified CaCO3 particles was 119.51º. Moreover, X-ray diffraction (XRD), FT-IR spectrums and thermogravimetry analysis (TGA) were employed to characterize the obtained products. The schematic illustration for interaction between the organic substrate and inorganic mineral in aqueous medium was showed in the end. The synthesized CaCO3 were applied to polyvinyl chloride (PVC) to improve its mechanical properties. The properties of PVC/CaCO3 composites have been tested



Corresponding author. Tel. +86-13944405698. E-mail: [email protected]. 1

ACCEPTED MANUSCRIPT such as tensile strength, impact strength, young modulus and SEM. Keywords: Hydrophobic; Calcium carbonate; DDP; Application; PVC

IP

T

1. Introduction

SC R

It is well known that calcium carbonate (CaCO3) is a natural occurring and abundant mineral comprising approximately 4% of the earth crust [1-4]. CaCO3 was used in many fields as a filler

NU

such as catalysis, electronics, medicine, pigments, rubbers, paper and so on [5-8]. The controlled chemical synthesis of inorganic materials with specific size, morphology and structure has

MA

attracted considerable attention because of the potential for design new materials and devices in various fields [9-11]. The key to the successful synthesis of an inorganic-organic composite is an

TE

D

understanding of the parameters that control the nucleation and growth of inorganic crystals under the organic substrate in aqueous solution [12-15]. In recent years, a considerable of attention and

CE P

effort have been devoted to investigate the calcium carbonate particles [16-20]. A promising approach is to use organic additives with complex functionalization patterns to control the

AC

nucleation, growth and alignment of inorganic materials through electrostatic matching and structured and stereochemical complementarity at inorganic / organic interface [21, 22]. Synthesis of CaCO3 is followed by two basic synthetic routes: (1) the solution route, through a double decomposition reaction, wherein aqueous CaCl2 and Na2CO3, or CaCl2 and (NH4)2CO3, or Ca(NO3)2 and Na2CO3 are combined in an equal molar ratio; and (2) the carbonation method, in which CO2 gas is bubbled through an aqueous slurry of Ca(OH)2. The carbonation method is preferred in terms of environment preservation and the effective use of mineral resources. The carbonation method is also an industrially useful method, but it is difficult for CaCO3 to control the crystal shape and modification [23, 24].

2

ACCEPTED MANUSCRIPT In this work, hydrophobic spherical aragonite CaCO3 nanoparticles were obtained in the presence of DDP. We attempted to study the crystallization of CaCO3 particles. The

IP

T

DDP-modified and the unmodified CaCO3 were applied in PVC to improve the tensile strength

SC R

and impact strength of PVC. It was advanced to use DDP which was made in the lab because the cost of the method was low in the industry.

NU

2. Experimental 2.1 Materials

MA

Dodecyl dihydrogen phosphate (DDP) was made by ourselves. Calcium oxide was of analytical reagent grade and made by Menghe Jiangsu Reagent Chemical Factory (China). They were

TE

D

analytical grade in this experiment. The distilled water used was made by us throughout the study. 2.2 Preparation of the hydrophobic spherical CaCO3 particles

CE P

The procedure employed for the preparation of CaCO3 was as follows. 10 g calcium oxide (CaO) was digested in 100 mL distilled water to form a calcium hydroxide (Ca(OH)2) slurry, which was

AC

kept for 12 h at least. The slurry was filtered through a 150 mesh sieve in order to get rid of the impurity and large particles. The ethanol solution of DDP was added into the slurry. The mixture was stirred vigorously for 1 h at 40 °C. Then the premixed CO2 and N2 with molar ratio of 3:10 were bubbled into the slurry through a column. The reaction should be stopped as soon as the pH value of the suspension decreased to 7.0. The obtained CaCO3 precipitates were rinsed firstly with anhydrous ethanol and hot distilled water three times, respectively. At last, the product was dried for at least 24 h in an oven at approximate 80 °C. 2.3 Preparation of DDP The cost of production in the industrialization of CaCO3 was an important parameter. The cost

3

ACCEPTED MANUSCRIPT of dodecyl dihydrogen phosphate (DDP) made by researchers was low. P2O5 was added into H3PO4 solution (the H3PO4 concentration is about 85%) under constant stirring at 50 °C. The

IP

T

solution was stirred for 1 h, then octadecyl alcohol (C18H37OH) was introduced into the system.

SC R

Meanwhile N2 was bubbled into the suspension in order that C18H37OH was not oxidized and the vapor was removed. After improving the temperature to 80 °C, the esterification reaction was maintained for 4 h, following extra P2O5 was put into the system in batches as complement to

NU

increase the yield of octadecyl dihydrogen phosphate (C18H37OPO3H2). The resulting suspension

2.4 Characterization of the samples

MA

was used as organic substrate.

D

Micrographs of the spherical CaCO3 particles were taken by a field emission scanning electron

TE

microscope (FESEM). It was carried out using a JEOL-JSM6700F at 15 kV. The crystalline phase

CE P

and structure of the synthesized CaCO3 were detected by X-ray diffraction (XRD) analysis with a Shimadju D/max-rA X-ray diffractometer with Cu Kα radiation, under the accelerating voltage 40

AC

kV, current 30 mA, and scanning rate 4° min−1. The contact angle was measured at 25 °C with a FTÅ200 (USA) contact angle analyzer. On flat solid surfaces, the contact angle could be measured by the sessile drop technique. The powdery samples (1 g) in 10 MPa pressure were first pressed into thin pellet and then the water droplet was dropped onto the pellet. The contact angle against water on a horizontal surface of a pellet was obtained. Fourier transform infrared spectroscopy (FT-IR) was performed on an Ominic System 2000 using KBr pellets. The thermogravimetry analysis (TGA) was performed on Melttler Toledo 825e instrument at 50-900 °C with a program heating rate of 10 °C min-1 in a flowing air atmosphere.

3. Results and discussion 4

ACCEPTED MANUSCRIPT 3.1 Effect of DDP on the morphologies and size of CaCO3 crystals FESEM images which showed the effect of DDP on the morphology of CaCO3 were presented

IP

T

in Fig.1. The effect of DDP on the morphology of CaCO3 was significant. Rhombus CaCO3

SC R

particles consisted of the plate-shaped crystals were obtained in the absence of DDP (Fig. 1(a)). However, it was evident that the mixture of the spherical and cubic CaCO3 crystals was obtained when the amount of DDP added reached 1 % (Fig. 1(b)). When the amount of DDP added was

NU

2 %, the morphology of CaCO3 particles changed greatly. The pure spherical CaCO3 particles with

MA

slick surfaces were observed as depicted in Fig. 1(c). The mean diameter of the spherical particles was about 40 nm. It was smaller than that in the Fig. 1(b). However, the mixture of cubic and

D

spherical CaCO3 particles was observed in Fig. 1(d) when the amount of DDP reached to 3 %.

CE P

during the reaction.

TE

Therefore it was important for the morphology of CaCO3 particles to control the amount of DDP

3.2 Effect of temperature on the morphology and size of CaCO3

AC

Fig. 2 showed FESEM micrographs of CaCO3 particles obtained at different reaction temperature. The effect of temperature on the morphology of CaCO3 was significant. The cubic CaCO3 particles were synthesized in the presence of DDP at 20 °C in Fig. 2(a). The mean size of the cube CaCO3 particles were about 40 nm. However, the spherical CaCO3 particles with smooth surface were obtained at 40 °C. The mean size of particles was about 30 nm (Fig. 2(b)). The shape was changed sharply at 60 °C in the Fig. 2(c). The spherical CaCO3 particles were decreased clearly and the cubic particles were increased. However, the spherical particles disappeared and only the congregations of irregular particles were observed at 80 °C in the Fig. 2(d).

5

ACCEPTED MANUSCRIPT The reaction temperature intensively affects the crystallization behaviors of the calcium carbonate polymorphs. High temperature is favorable to the nucleation of aragonite crystal in

IP

T

super saturation solution. Aragonite is usually achieved at a higher temperature than 50 ºC using

SC R

a solution method of preparation [25]. In this work, we concluded that aragonite particles could be produced when the reaction temperature was higher than 40 ºC. Although the fraction of aragonite in the resulting precipitates was gradually improved with increasing the reaction

NU

temperature, the products were all the same of a mixture of aragonite and calcite. Actually, at the

MA

initial carbonation stage, aragonite crystals and calcite crystals nucleate simultaneously and competitively, therefore, harvesting an absolutely pure aragonite phase is impossible in this

D

system.

TE

3.3 XRD patterns of the obtained CaCO3 particles

CE P

Fig. 3 was the XRD patterns of CaCO3 obtained at different temperatures in the presence of DDP in the system. It found that there was most of calcite in the precipitates when the reaction

AC

temperature was 20 °C (Fig. 3(a)). XRD of the washed precipitates gave distinct peaks that were characteristic of the (012), (104), (110), (202) and (116) planes, consistent with pure calcite crystals. These peaks were centered at 2θ=23.04°, 29.40°, 36.00°, 43.16° and 48.50°, respectively. When increasing the reaction temperature to 40 °C, 60 °C and 80°C (Fig. 3(b)-(d)), the typical peaks of aragonite phase were strengthened such as (111), (012) and (221) planes. Furthermore, with increasing the reaction temperature, the fraction of aragonite in the resulting precipitates was gradually improved. The products were of a mixture of aragonite and calcite. Furthermore, with increasing the reaction temperature, the fraction of aragonite in the resulting precipitates was gradually improved.

6

ACCEPTED MANUSCRIPT Especially, the (104) planes was weakened obviously. The polymorphic ratio of aragonite and calcite in precipitated CaCO3 was calculated by the following equation derived from a calibration

IP

T

curve, which was obtained from crystal mixtures with known ratios of polymorphs: y=1−1/ (1+3.9

SC R

Ia / Ic), where y was the calculated weight fraction of aragonite, and Ia and Ic were the integrated intensity of the XRD spectra characteristic of the aragonite (111) peak and the calcite (104) peak, respectively[26]. The calculated result showed that the fraction of aragonite was 0.503, 0.699,

NU

0.757 and 0.787 when the temperature was changed form 20 °C to 80 °C.

MA

Aragonite is thermodynamically metastable phase. Without any additives, it is well-known that aragonite completely transforms into the most thermodynamically stable calcite in the aqueous

D

solution[27-29]. Increasing the reaction temperature cannot enable the aragonite phase to become

TE

thermodynamically stable phase in the absence of DDP. It means that higher temperature is

CE P

obviously favorable to the nucleation of aragonite crystal, but not the crucial factor of stabilizing it. We speculate that the aragonite crystals in the resulting precipitates were stabilized by DDP to

AC

prevent phase transformation.

3.4 Effect of the mass ratio of DDP on contact angle Fig. 4 was showed the effect of the mass ratio of DDP to CaCO3 on contact angle. The interaction characteristics of the obtained CaCO3 particles surfaces were measured by the contact angle. Fig. 4 (a) indicated that with the increasing of the mass ratio of DDP to CaCO3, the contact angle of CaCO3 particles increased gradually. When the mass ratio was 2 %, the contact angle was 119.51°. It proved that when the mass ratio of DDP to CaCO3 was higher than 2 %, the CaCO3 particles had hydrophobic property. The conclusion was obtained that the optimum molar ratio of DDP to CaCO3 is 2 % at 40 °C by the information provided in Fig. 1. Therefore, it could be drawn

7

ACCEPTED MANUSCRIPT the conclusion that the obtained CaCO3 particles were of good hydrophobic property. The contact angles of the pellets after drying at 100°C for 24 h were not changed, indicating that no volatile

IP

T

compounds are present in the samples.

SC R

3.5 FT-IR characterization of spherical CaCO3

Fig. 5 showed FT-IR spectra of the CaCO3 particles nucleated in the absence (Fig. 5(a)) and in the presence of DDP (Fig. 5(b)). The spectra confirmed the formation of calcite with characteristic

NU

absorption bands observed at 716 cm–1, 872 cm–1 and 1502 cm–1, corresponding to the ν4, ν2 and ν3

MA

CO32– absorption bands of calcite [30]. Weak bands were also observed at 2979 cm–1and 2855 cm–1 which were associated with asymmetric and symmetric methyl and ethylene C–H stretches,

D

respectively. This suggestted that surfactant molecules remained strongly associated with the

TE

CaCO3 crystals even after extensive washing.

CE P

3.6 TGA characterization of spherical CaCO3 The TGA curves for CaCO3 particles which were obtained in the absence and in the presence of

AC

DDP were indicated in Fig.6. It could be obviously seen that a larger weight loss occurred in the temperature range from 200 ˚C to 620 ˚C, which was attributed to the thermal decomposition of organic substrates in the CaCO3 powders. We could observe that the weight loss of the products from the curve b was about 5.1 wt. %. Another stage was from 620 ˚C to 755 ˚C, where the largest mass loss was observed. This could be assigned to the thermal decomposition of calcite (CaCO3 → CaO + CO2  ). 3.7 Monitoring of the pH value during experiment In this work, the change of the pH value was monitored during experiment by the pH meter. Fig. 7 indicated the changes in pH value with bubbling time for 13.0 wt.% Ca(OH)2 at a 1.5 L/min CO2

8

ACCEPTED MANUSCRIPT gas flow rate in the absence and in the presence of DDP. The pH of all the suspensions starts from a high basic value of about 12.5. In the absence of DDP, the high basic pH was maintained for

IP

T

about 90 min before dramatically dropping to a value of 7. However, the high basic pH value

SC R

dramatically dropped to 7 after 45 min in the presence of DDP. A number of researchers have observed this typical pH behavior which exhibits two distinct regions: a constant rate of absorption period and a falling rate period. During the constant rate period, the aqueous phase was

NU

always kept saturated with OH− ions and the most of the Ca(OH)2 conversion to carbonate was

MA

completed during this period. The effect of DDP increased the retention time and contact area of CO2 in the solution thus the higher carbonation efficiency was observed. From the results, we

D

could conclude that the presence of DDP accelerates the period of absorption and shortens the

TE

time of carbonation. It was potential useful in industry.

CE P

3.8 Reaction mechanism Analysis

In the work, the DDP solution was added to the Ca(OH)2 slurry using a mechanical stirrer. Fig.

AC

8 showed the schematic illustration for interaction between the organic substrate and inorganic mineral in aqueous medium. This reaction consisted of three stages. First, interfacial recognition in the interface of organic /inorganic: Ca2+ ions of Ca(OH)2 reacted with DDP to form a hydrophobic salt of C12H25OPO3Ca. Then crystal nucleation and growth: CO2 gas was introduced into the stirred mixture at 40 °C to synthesize CaCO3. The hydrophobic properties of the final CaCO3 particles were attributed to the deposition of the resulted C12H25OPO3Ca onto the surface of CaCO3. Final, mineralization arrest and self-assembly: nucleation of crystals was induced by the absorption of organic substrates on the CaCO3 particles surface. 3.9 Applied properties of the modified calcium carbonate

9

ACCEPTED MANUSCRIPT 3.9.1 Tensile strength and impact strength of PVC/CaCO3 composites The equipments were used such as high speed blunger, twin-screw extruder, universal sample

IP

T

testing machine and charpy impact tester in the test. The test was performed according to Table 1.

SC R

The mechanical properties were the important parameters of the materials. When CaCO3 modified by DDP as a filler was used in PVC, the mechanical properties of the products would be enhanced such as tensile strength and impact strength. Fig.9 showed that the effect of unmodified

NU

and modified CaCO3 on the tensile property in PVC. The results indicated that the tensile strength

MA

was increased first and then decreased in the picture when CaCO3 particles were synthesized in the absence of organic substrate (Fig.9a) and in the presence of DDP (Fig.9b). When the CaCO3

D

loading was 5%, the maximum tensile strength was 18.75 MPa. However, the unmodified-CaCO3

TE

of tensile strength was 14.89 MPa only. The highest measured PVC properties were observed for

CE P

CaCO3 with DDP-modified nanoparticles, where an increase in tensile strength (+26%). In the meantime, the result was observed that the elongation at break was improved by 89%, indicating

AC

the high toughness.

Previous work had shown that with addition of the substance could be obtained [31-33]. The effect of unmodified and modified CaCO3 on the impact property in PVC was shown in Fig.10. The results indicated that the impact strength was increased first and then decreased in the picture when CaCO3 particles were synthesized in the absence of organic substrate (Fig.10a) and in the presence of DDP (Fig.10b). When the CaCO3 loading is 5%, the maximum impact strength was 53.1kJ/m2. However, the unmodified-CaCO3 of impact strength was 15.2kJ/m2 only. The highest measured PVC properties were observed for CaCO3 with DDP-modified nanoparticles, where an increase in tensile strength (+249%). From the above discussion, the conclusion was drawn that

10

ACCEPTED MANUSCRIPT the properties of DDP-modified CaCO3 particles was superior to the unmodified-CaCO3 particles in PVC.

IP

T

3.9.2 Young modulus values of PVC/CaCO3 composites

SC R

In our work, the impact strength was increased first and then decreased in absence and in the presence of DDP. It could be connected with the rigidity of filler and the strong interaction between the filler and polymer matrix. At the same time, the young modulus values were

NU

calculated in the test. The literature on the effect of surface treatment on young modulus was

MA

contradictory. In some cases an increase was observed [34], occasionally no changes were reported [35], or even a decrease in modulus was claimed after treatment [36]. According to our

D

work the influence of the surface treatment on young modulus is not obvious. As shown in Fig. 11,

TE

the young modulus values of unmodified-CaCO3 and DDP-modified CaCO3 composites increased

CE P

simultaneously with the increase of CaCO3 content independent of the filler dispersion state. 3.9.3 SEM micrographs of PVC/CaCO3 composites

AC

The size and morphology of modified CaCO3 particles play an important role on the property of PVC. At the same time the quality of PVC have an important effect on the test result. The SEM micrographs of the tensile-fractured surfaces of the composites were shown in Fig. 12. The figure of pure PVC was seen in Fig. 12(a). As seen in Fig. 12(b), some cavities could be found on the fracture surface of the composites when the fraction of CaCO3 was 5. It indicated that the CaCO3 particles and PVC were combined well. However, few cavities were observed on the fracture surface of PVC/CaCO3 composites, as shown in Fig. 12(c) and Fig. 12(d). The presence of CaCO3 particles must be responsible for the cavitations. These cavitations could absorb large amounts of energy, leading to the improvement of the composites’ tensile strength. Chan also found

11

ACCEPTED MANUSCRIPT cavitations on the fracture surface of PP/CaCO3 composites [37]. This indicates that the toughening effect of CaCO3 on pure PVC was restricted to the mechanical coupling between the

IP

T

filler and polymer matrix, and no cavitations are involved.

SC R

4. Conclusions

In conclusion, the spherical CaCO3 particles could be synthesized by a simple carbonation

NU

method in the presence of DDP as a modifier. The optimal reaction temperature was 40°C and the amount of DDP was 2%. It could come to conclusion that DDP plays an important role of control

MA

on the nucleation, growth and alignment of CaCO3 particles in the reaction process. The properties of DDP-modified CaCO3 particles were superior to the unmodified-CaCO3 particles in PVC. The

CE P

Acknowledgement

TE

D

obtained spherical hydrophobic CaCO3 particles could find applications in industrial field.

This research was financed by the National Natural Science Foundation of China (51404108)

China.

AC

and Scientific Research Innovation Plan for Young Talented Person of Jilin Normal University,

References

[1] Y. Ueno, H. Futagawa, Y. Takagi, A. Ueno, Y. Mizushima, Control of crystal nucleation and growth of calcium carbonate by synthetic substrates, J Controlled Release. 103(2005)93−98. [2] J. Liu, S. Pancera, V. Boyko, J. Gummel, R. Nayuk, K. Huber, Impact of sodium polyacrylate on the amorphous calcium carbonate formation from supersaturated solution, Langmuir. 28(2012)3593−3605. [3] F. Erika, B. Pukánszky, A. Tóth, I. Bertóti, Surface modification and characterization of

12

ACCEPTED MANUSCRIPT particulate mineral fillers, J Colloid Interface Sci. 135(1990)200–204. [4] A.F. Wallace, L.O. Hedges, F.M. Alejandro, P. Raiteri, J.D. Gale, G.A. Waychunas, S.

IP

T

Whitelam, J.F. Banfield, Y.J.J. De, Microscopic evidence for liquid-liquid separation in

SC R

supersaturated CaCO3 solutions. Science, 341(2013)885−889.

[5] S. Thachepan, M. Li, S. Davis, Additive-mediated crystallization of complex calcium carbonate superstructures in reverse microemulsions, J Chem. Mater. 18(2006)3557–3561.

NU

[6] Y. Liu, Y.J. Cui, H.Y. Mao, R. Guo, Calcium carbonate crystallization in the presence of

MA

casein, Cryst. Growth Des. 12(2012)4720−4726.

[7] H.P. Mattila, I. Grigaliūnaitė, R. Zevenhoven, Chemical kinetics modeling and process

D

parameter sensitivity for precipitated calcium carbonate production from steelmaking slags,

TE

Chemical Engineering Journal. 192(2012)77–89.

CE P

[8] W. Li, L. Liu, W. Chen, L. Yu, W. Li, H. Yu, Calcium carbonate precipitation and crystal morphology induced by microbial carbonic anhydrase and other biological factors, Process

AC

Biochemistry. 45(2010) 1017–1021. [9] W.Y. Zhang, Y. Hu, L.J. Xi, Y.J. Zhang, H.C. Gu, T. Zhang, Preparation of calcium carbonate

superfine

powder

by

calcium

carbide

residue,

Energy

Procedia.

17(2012)1635–1640. [10] A.T. Nagaraja, S. Pradhan, M.J. Mcshane, Poly (vinylsulfonic acid) assisted synthesis of aqueous solution stable vaterite calcium carbonate nanoparticles, Journal of Colloid and Interface Science. 418(2014)366–372. [11] C.Y. Wang, Control the polymorphism and morphology of calcium carbonate precipitation from a calcium acetate and urea solution, Mater. Lett. 62(2008)2377–2380.

13

ACCEPTED MANUSCRIPT [12] H. Trana, L. Tranb, H. Vua, H. Thai, Facile surface modification of nanoprecipitated calcium carbonate by adsorption of sodium stearate in aqueous solution, Colloids and Surfaces A:

IP

T

Physicochem. Eng. Aspects. 366(2010) 95–103.

SC R

[13] A.L. Kabalah, B. Mayze, Y. Kauffmann, A.N. Fitch, L. Bloch, P.U.P.A. Gilbert, B. Pokroy, Vaterite crystals contain two interspersed crystal structures, Science. 340(2013) 454–458. [14] S.Q. Bai, G.W. Naren, M. Nakano,Y. Okaue, T. Yokoyama, Effect of polysilicic acid on the

NU

precipitation of calcium carbonate, Colloids and Surfaces A: Physicochem. Eng. Aspects. 445

MA

(2014)54–58.

[15] Y. Chen, X. Ji, G. Zhao, X. Wang, Facile preparation of cubic calcium carbonate

TE

200(2010)144–148.

D

nanoparticles with hydrophobic properties via a carbonation route, Powder Technology.

CE P

[16] X. Chen, Y.C. Zhu, Y.P. Guo, B. Zhou, X. Zhao, Y.Y. Du, H. Lei, M. Li, Z.C. Wang, Carbonization synthesis of hydrophobic CaCO3 at room temperature, Colloids Surf. A. 353

AC

(2–3)(2010)97–103.

[17] O. Grassmann, P. Lobmann, Biomimetic nucleation and growth of CaCO3 in hydrogels incorporating carboxylate groups, Biomaterials. 25(2004)277–282. [18] C. Wang, C. Piao, X. Zhai, F. Hickman, J. Li, Synthesis and characterization of hydrophobic calcium carbonate particles via adodecanoic acid inducing process, Powder Technology. 198(2010)131–134. [19] S. Kirboga, M. Öner, Application of experimental design for the precipitation of calcium carbonate in the presence of biopolymer, Powder Technology. 249(2013)95−104. [20] Y. Levi-Kalisman, G. Falini, L. Addadi, Structural differences between biogenic amorphous

14

ACCEPTED MANUSCRIPT calcium carbonate phases using X-ray absorption spectroscopy, Struct Boil. 135(2001)8–13. [21] H. Xu, S.C. Zhou, X.B Jin, Y.D. Liu, Monte carlo simulation of the induction time and

IP

T

particle size distribution in the nucleation of calcium carbonate, Powder Technology. 253

SC R

(2014)242–246.

[22] S. Li, L. Yu, G. Fei, L. Shi, L Zheng, S. Yuan, Facile preparation of diversified patterns of calcium

carbonate

in

the

presence

DTAB,

Journal

of

Crystal

Growth.

NU

312(2010)1766–1773.

of

MA

[23] S. Eloneva, A. Said, C. J. Fogelholm, R. Zevenhoven, Preliminary assessment of a method utilizing carbon dioxide and steelmaking slags to produce precipitated calcium carbonate,

D

Applied Energy. 90(2012)329–334.

TE

[24] K.N. Islam, M.Z.B.A. Bakar, M.M. Noordin, M.Z.B. Hussein, N.S.B.A. Rahman, M.E. Ali,

CE P

Characterization of calcium carbonate and its polymorphs from cockle shells (Anadara granosa), Powder Technology. 213(2011)188–191.

AC

[25] G. Yan, L. Wang, J. Huang, The crystallization behavior of calcium carbonate in ethanol/water solution, Powder Technol. 192 (2009) 58–64. [26] N. Wada, M. Okazaki, S. Tachikawa, Effects of calcium-binding polysac-charides from calcareous algae on calcium carbonate polymorphs under conditions of double diffusion, J. Cryst. Growth. 132 (1993) 115-122. [27] M.M.M.G.P.G. Mantilaka, H.M.T.G. A. Pitawala, R.M.G. Rajapakse, D.G.G.P. Karunaratne, K.G.U. Wijayantha, Formation of hollow bone-like morphology of calcium carbonate on surfactant/polymer templates, Journal of Crystal Growth. 392 (2014) 52–59. [28] P. Bots, L.G. Benning, J. Rodriguez-Blanco, T. Roncal-Herrero, S. Shaw, Mechanistic insights

15

ACCEPTED MANUSCRIPT into the crystallization of amorphous calcium carbonate (ACC), Cryst. Growth Des. 12(2012) 3806−3814.

IP

T

[29] D. Zhao, J. Jiang, J. Xu, L. Yang, T. Song, P. Zhang, Synthesis of template-free hollow

SC R

vaterite CaCO3 microspheres in the H2O/EG system, Mater. Lett. 104(2013) 28–30. [30] K.N. Islam, M.Z.B.A. Bakar, M.E. Ali, M.Z.B. Hussein, M.M. Noordin, M.Y. Loqman, G. Miah, H. Wahid, U. Hashim, A novel method for the synthesis of calcium carbonate

NU

(aragonite) nanoparticles from cockle shells[J]. Powder Technology. 235(2013)70–75.

MA

[31] N. Chen, C.Y. Wan, Y. Zhang, Y.X. Zhang, Effect of nano-CaCO3 on mechanical properties of PVC and PVC/Blendex blend, Polymer Testing. 23 (2004) 169–174.

D

[32] Z. Demjén, B. Pukánszky, J Nagy, Evaluation of interfacial interaction in polypropylene/

TE

surface treated CaCO3 composites, Composites Part A. 29A (1998) 323–329.

CE P

[33] X.H. Chen, C.Z. Li, S.F. Xu, L. Zhang, W. Shao, H.L. Du, Interfacial adhesion and mechanical properties of PMMA-coated CaCO3 nano-particle reinforced PVC composites,

AC

China Particuology. 4 (2006)25–30. [34] K. Okuno, R.T. Woodhams, Mica reinforced polypropylene, Polym. Eng. Sci. 15(1975)308–315. [35] V.P. Juskey, C.E. Chaffey, J. Canadian, Rheology and tensile properties of polypropylene reinforced with glycerol-treated mica, Chem. Eng. 1982, 60, 334–341. [36] A.S. Kenyon, H.J. Duffey, Polym. Properties of a particulate-filled polymer, Eng. Sci. 7(1967)189–196. [37] C.M. Chan, J. Wu, J.X. Li, Y.K. Cheng, Polypropylene/calcium carbonate nanocomposites, Polymer. 43(2002)2981–2992.

16

SC R

IP

T

ACCEPTED MANUSCRIPT

NU

Fig. 1 FESEM images of the as-prepared CaCO3 particles in the presence of DDP: (a) 0, (b) 1 %, (c) 2 % and (d)

AC

CE P

TE

D

MA

3 %.

17

NU

SC R

IP

T

ACCEPTED MANUSCRIPT

Fig. 2 FESEM of CaCO3 particles obtained at the different temperature in the presence of DDP: (a) 20 °C; (b)

AC

CE P

TE

D

MA

40 °C; (c) 60 °C; (d) 80°C.

18

ACCEPTED MANUSCRIPT

(c)

aa

a

a

aa

a

a

a

a

aa 25

30

35

NU

20

SC R

(b)

(a)

c202 a221 c116

T

a111 c104 a012 c110 a112 c012 a021

aragonite calcite

IP

(d)

a c

40

45

50

55

2 Theta (degree)

MA

Fig. 3 XRD patterns of CaCO3 particles obtained at the different temperature in the presence of DDP: (a) 20 °C; (b)

AC

CE P

TE

D

40 °C; (c) 60 °C; (d) 80 °C.

19

ACCEPTED MANUSCRIPT

(a)

120

T IP

80

60

40

20

0 0.0

0.5

1.0

1.5

SC R

o

Contact angle ( )

100

2.0

2.5

CE P

TE

D

MA

NU

Mass ratio of DDP to CaCO3(%)

AC

Fig. 4 Effect of the mass ratio DDP to CaCO3 on contact angle (a) and the measurement of CaCO3 prepared in the presence of DDP (2%) (b).

20

ACCEPTED MANUSCRIPT

T IP

1502

716

SC R

b

872

2979 2855

Transmittance

a

3000

2500

2000

1500

NU

3500

1000

500

-1

Wavenumber (cm )

AC

CE P

TE

D

MA

Fig. 5 FT-IR spectra of obtained CaCO3 particles in the absence of DDP (a) and in the presence of DDP(b).

21

ACCEPTED MANUSCRIPT

100

T IP

80

70

60

SC R

Wight loss (%)

90

a b

50 100

200

300

400

500

600 o

700

NU

Temperature ( C)

800

900

AC

CE P

TE

D

MA

Fig. 6 TGA cures of obtained CaCO3 particles in the absence of DDP (a) and in the presence of DDP(b).

22

ACCEPTED MANUSCRIPT

13 12

T

10

IP

pH

11

8

b 7 0

20

40

60

SC R

9

a

80

100

120

The reaction time (min)

AC

CE P

TE

D

MA

NU

Fig. 7 Change of pH VS carbonation time (a) in the absence of DDP; (b) in the presence of DDP.

23

NU

SC R

IP

T

ACCEPTED MANUSCRIPT

MA

a: Interfacial recognition in the interface of organic/inorganic; b: Crystal nucleation and growth; c: Mineralization arrest and self-assembly. Fig.8 Schematic illustration for interaction between the organic substrate and inorganic mineral in aqueous

AC

CE P

TE

D

medium.

24

ACCEPTED MANUSCRIPT

260

a

280

13.4

160 140

13

143 12.3

120

T

180

14

17 16 15

13

100 12

12

0

5

10

15

20

25

30

15.3

0

5

10

15

240

200 180

146

14

260

220

IP

200 209

Tensile strength (MPa)

15.1

Tensile strength The elongation at break

160 159

140

The elongation at break (%)

15

264

18

The elongation at break (%)

220

18.7

b

240

Tensile strength The elongation at break

Tensile strength (MPa)

19

235

SC R

16

120 12.7 20

100 25

30

The CaCO3 loading (%)

The CaCO3 loading (%)

NU

Fig. 9 Effect of the CaCO3 loading on tensile strength and the elongation at break in PVC (a:

AC

CE P

TE

D

MA

unmodified-CaCO3(SD=1.257, n=4); b: DDP-modified CaCO3(SD=1.334, n=4)).

25

ACCEPTED MANUSCRIPT

60

T

53.2

30

20.5 20

19.6 10

12.9

0 0

5

10

SC R

40

12.7

NU

Impact strength ( kJ/m

2

IP

50

15

20

5.0 25

30

MA

The CaCO3 loading (%)

Fig. 10 Effect of the CaCO3 loading on impact strength in PVC (SD=0.35, n=4) (a: unmodified-CaCO3; b:

AC

CE P

TE

D

DDP-modified CaCO3).

26

ACCEPTED MANUSCRIPT

5.0

PVC/ unmodified CaCO3 PVC/DDP-modified CaCO3

T IP

4.0

3.5

SC R

Young Modulus(GPa)

4.5

3.0

NU

2.5

2.0 5

10 15 20 The content of CaCO3(phr)

MA

0

AC

CE P

TE

D

Fig.11 Young modulus values of PVC/CaCO3 composites (SD=0.2, n=4).

27

25

30

SC R

IP

T

ACCEPTED MANUSCRIPT

Fig.12 SEM figures of PVC/CaCO3 composites (a) pure PVC; (b) PVC/CaCO3 (5 phr); (c) PVC/CaCO3 (10 phr);

AC

CE P

TE

D

MA

NU

(d) PVC/CaCO3 (30 phr).

28

ACCEPTED MANUSCRIPT

The type of material

The name of material

The dosage of material/Phr

Polyvinyl chloride

PVC

100

Heat stabilizer

Calcium stearate

T

Table 1 The design of formula

Lubricant

Paraffin wax

Impact modifier

CPE

Processing agent

ACR

IP

1.0

AC

CE P

TE

D

MA

NU

SC R

2.0

29

4.0 1.5

ACCEPTED MANUSCRIPT

AC

CE P

TE

D

MA

NU

SC R

IP

T

Graphical Abstract

30

ACCEPTED MANUSCRIPT Highlights

IP

2. The contact angle of hydrophobic CaCO3 particles was 119.51º.

T

1. Hydrophobic spherical CaCO3 particles were prepared via a DDP inducing process.

SC R

3. The polymorphs were characterized with XRD, FT-IR and TGA.

4. The schematic illustration of the reaction was discussed in the end.

AC

CE P

TE

D

MA

strength, young modulus and SEM.

NU

5. The properties of PVC/CaCO3 composites have been tested such as tensile strength, impact

31