Effects of anions on calcium arsenate crystalline structure and arsenic stability

Effects of anions on calcium arsenate crystalline structure and arsenic stability

Accepted Manuscript Effects of anions on calcium arsenate crystalline structure and arsenic stability Jie Lei, Bing Peng, Yan-Jie Liang, Xiao-Bo Min,...

2MB Sizes 0 Downloads 14 Views

Accepted Manuscript Effects of anions on calcium arsenate crystalline structure and arsenic stability

Jie Lei, Bing Peng, Yan-Jie Liang, Xiao-Bo Min, Li-Yuan Chai, Yong Ke, Yang You PII: DOI: Reference:

S0304-386X(17)30753-3 doi:10.1016/j.hydromet.2018.03.007 HYDROM 4771

To appear in:

Hydrometallurgy

Received date: Revised date: Accepted date:

13 September 2017 31 January 2018 6 March 2018

Please cite this article as: Jie Lei, Bing Peng, Yan-Jie Liang, Xiao-Bo Min, Li-Yuan Chai, Yong Ke, Yang You , Effects of anions on calcium arsenate crystalline structure and arsenic stability. The address for the corresponding author was captured as affiliation for all authors. Please check if appropriate. Hydrom(2017), doi:10.1016/ j.hydromet.2018.03.007

This is a PDF file of an unedited manuscript that has been accepted for publication. As a service to our customers we are providing this early version of the manuscript. The manuscript will undergo copyediting, typesetting, and review of the resulting proof before it is published in its final form. Please note that during the production process errors may be discovered which could affect the content, and all legal disclaimers that apply to the journal pertain.

ACCEPTED MANUSCRIPT Effects of anions on calcium arsenate crystalline structure and arsenic stability Jie Leia, Bing Penga, b, Yan-Jie Lianga,b,c,*, Xiao-Bo Mina,b,*, Li-Yuan Chaia,b, Yong Kea,b, Yang Youa

Institute of Environmental Science and Engineering, School of Metallurgy and

PT

a

Chinese National Engineering Research Center for Control & Treatment of Heavy

SC

b

RI

Environment, Central South University, Changsha, Hunan 410083, China

c

NU

Metal Pollution, Changsha, Hunan 410083, China

Xiang Guang Copper Co., Ltd., Yang gu, Shandong, 252327, China

MA

*Corresponding authors at: Institute of Environmental Science & Engineering, School of

D

Metallurgy and Environment, Central South University, Changsha, Hunan 410083, China.

AC

CE

PT E

E-mail addresses: [email protected] (Y.-J. Liang), [email protected] (X.-B. Min).

ACCEPTED MANUSCRIPT

Abstract Based on the crystallization reaction between calcium and arsenate, three anions, namely, chloride (Cl-), sulfate (SO42-), and carbonate (CO32-), were introduced during the formation of calcium arsenate in this study. The effects of these anions on arsenic

PT

stability and calcium arsenate crystalline properties were characterized using TCLP,

RI

XRF, XRD, SEM-EDS, TEM and particle size distribution (PSD). The results show

SC

that these anions significantly affect the calcium arsenate crystalline structure and

NU

arsenic-leachate concentration. The effect of chloride on arsenic stabilization was mainly a result of the formation and growth of calcium arsenate apatite

MA

(Ca5(AsO4)3OH and Ca5(AsO4)3Cl) crystal. Sulfate is propitious to improve the formation of Ca4(OH)2(AsO4)2·4H2O crystals and enhance their stability effectively

PT E

D

under corresponding sulfate concentration treatments. A small amount of carbonate is beneficial to the formation and growth of Ca4(OH)2(AsO4)2·4H2O crystals. However,

CE

when the CO32- concentration was higher than 0.5 mol/L, Ca-As compounds were not precipitated. Instead, CaCO3 and Na3Ca(CO3)2·5H2O were generated successively,

AC

inhibiting calcium-arsenate crystallization and thus releasing more arsenic into aqueous solution. The trends of grain size are opposite to that of arsenic-leachate concentration, indicating that larger calcium arsenate crystals are more stable in the TCLP test. The internal structure of different Ca-As compounds can be changed and transformed by adding the three anions within a certain range. In summary, the results

ACCEPTED MANUSCRIPT

of this paper provide some meaningful information for the treatment of arsenic-containing wastewater or arsenic-bearing sludges using lime precipitation. Keywords: High arsenic-bearing sludge; Calcium arsenate crystallization; Anions,

AC

CE

PT E

D

MA

NU

SC

RI

PT

Arsenic-leachate concentration; Grain size; Lime precipitation.

ACCEPTED MANUSCRIPT

1. Introduction Arsenic is one of the most toxic metalloid found in industrial wastewater which has caused increasing public concern (Wang et al. 2011; Wu et al. 2016). Lime precipitation is used widely in arsenic-bearing wastewater treatment because of its

PT

low cost and simple process (Chen et al. 2015; Li et al., 2011). However, this process

RI

generates a large amount of arsenic sludge, which is classified as hazardous waste due

SC

to its high arsenic content (Cui et al., 2014; Fei et al., 2017; Min et al., 2017; Morales

NU

et al., 2010). Various types of technologies, such as cementation (Choi et al., 2009; Li et al., 2017; Randall, 2012), polymeric encapsulation (Shaw et al., 2008),

MA

hydrothermal precipitation (Vinals et al., 2010; Peng et al., 2017), mineralization (Chai et al., 2017), co-treatment solidification (Li et al., 2016; Liu et al., 2017),

PT E

D

mechanical milling (Liang et al., 2017) and vitrification (Zhao et al., 2017), have been developed to reduce the mobility of arsenic and other heavy metals in the sludge.

CE

Calcium arsenate crystallization is one of the most common methods for reducing arsenic-leachate concentration from the arsenic-bearing precipitates (Donahue and

AC

Hendry, 2003). Arsenic-leaching behavior is mainly affected by the solubility and phase-transfer of the arsenic compounds (Ke et al., 2017; Ozverdl and Erdem, 2010; Xie et al., 2013). Many researchers have shown that lime addition reduces As mobility in contaminated slurries due to the formation of low-solubility Ca-As precipitates such as Ca4(OH)2(AsO4)2·4H2O and Ca5(AsO4)3OH (Bothe and Brown, 1999; Camacho et al., 2009; Lei et al., 2017).

ACCEPTED MANUSCRIPT

It is well known that arsenic-containing wastewater often contains multiple anions such as Cl-, SO42-, and CO32-. It has been proven that these anions have a significant influence on arsenic precipitation (Meng et al., 2002; Rivas et al., 2012; Sun et al., 2017; Welham et al., 2000). There are studies that show chloride can enhance arsenic

PT

removal through the nano-zero-valent iron process (Tanboonchuy et al., 2012). Other

RI

studies have found that sulfate has different effects on arsenate removal under

SC

different concentrations (Sun et al., 2006, Zhang et al., 2008). Calcium arsenate

NU

precipitate formed as a result of lime addition is not stable, because it can decompose to calcium carbonate and release arsenic under an attack of atmospheric CO2 which is

MA

easily converted to carbonate (Luo et al., 2010). However, CO2 combined with ferrous is used to evaluate arsenic immobilization in red mud, and the aqueous arsenic

PT E

D

concentration effectively decreased (Li et al, 2012). Consequently, these anions may play an important role in the removal and immobilization of arsenic and other heavy

CE

metals.

However, the influence of these anions on arsenic immobilization has not been

AC

systematically studied. In fact, the properties and stability of crystals are susceptible to anions during the process of crystallization (Crundwell, 2016). Previous studies have demonstrated that sulfate ions can distort calcite structure when incorporated into the calcite crystal lattice (Kontrec et al., 2004). Merely changing the anion types and dosages can also affect the rate of formation and crystalline structure of the synthetic compounds (Petrik et al., 2009). Hence, the objective of this study was to

ACCEPTED MANUSCRIPT evaluate the effects of anions such as Cl-, SO42- and CO32- on the formation and growth of calcium arsenate crystals and to reveal the relationship between arsenic stability and crystal structure. The results can provide useful information on the

arsenic-containing wastewater based on lime precipitation.

RI

2. Materials and methods

PT

process of arsenic sludge treatment based on calcium arsenate crystallization or high

SC

2.1. Materials

NU

Calcium hydroxide (Ca(OH)2), nitric acid (HNO3), sulfuric acid (H2SO4), glacial acetic acid (CH3COOH), sodium arsenate (Na3AsO4·12H2O) over 99%, sodium

MA

chloride (NaCl), sodium sulfate (Na2SO4) and sodium carbonate (Na2CO3) were purchased from the Sinopharm Chemical Reagent Company Limited in China. All the

PT E

D

reagents were of analytical grade, and all the dilutions were made using high-purity de-ionized water (18 MΩ cm-1 resistivity) obtained from a mole analytical ultrapure

CE

water system (Molecular, Molresearch 1010A, China). The bottles and glassware used for storing samples were washed in 10% (v/v) HNO3 for 24 h and rinsed with

AC

ultrapure water to avoid the effects of impurities. 2.2. Experimental procedure A schematic diagram of the experimental set up is shown in Fig. 1. The crystallization experiments were performed in 500-mL flasks containing a mixture of Ca(OH)2 and Na3AsO4·12H2O in a 2.0:1 Ca/As molar ratio and 4.0:1 liquid/solid mass ratio under stirring with a glass rod for 2 min. The initial pH value of the

ACCEPTED MANUSCRIPT

mixture was detected using a pH meter (Mettler-Toledo, FE20). The mixture was reacted on a magnetic stirring apparatus at 25°C for 5 h. The precipitates were separated using a vacuum filter, washed with de-ionized water three times, oven-dried

AC

CE

PT E

D

MA

NU

SC

RI

PT

at 60°C for 24 h, and then subjected to characterization and a leaching toxicity test.

PT

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

MA

NU

SC

RI

Fig. 1. Schematic diagram of the experimental procedure.

ACCEPTED MANUSCRIPT

2.3. Characterization A leaching toxicity test was conducted to evaluate the arsenic-leaching behavior of calcium-arsenic compounds according to the toxicity characteristic leaching procedure (TCLP, USEPA SW-846, Method 1311) (USEPA, 1992), which is the

PT

current USEPA protocol for determining whether waste is hazardous. The chemical

RI

composition of precipitates was detected using an X-ray fluorescence spectrometer

SC

(XRF, Shimadzu-1800, operated at 40 kV, 95 mA). The phase and crystallinity of all

NU

samples were characterized using X-ray diffraction (XRD, Rigaku D/MAX 2550 VPC diffractometer, 40 kV, 20 mA). The average grain size of the crystals was calculated

MA

using the Scherrer equation as follows (Min et al., 2013): (1)

PT E

D

where d is the average grain size; k is the Scherrer constant, taken to be 0.89; λ is the wavelength of the X-ray (0.15418 nm); β is the corrected half-width of the diffraction

CE

peak; and θ is the diffraction peak angle. In addition, scanning electronic microscope coupled by energy dispersive

AC

spectroscopy (SEM-EDS, Nova Nano SEM 230), laser particle size analyser (OMEC LS-POP VI) and a transmission electron microscope (TEM, JEM-2100F) were used to observe the morphological features and surface characteristics of the Ca-As precipitates, respectively.

ACCEPTED MANUSCRIPT

3. Results and discussion 3.1 Characterization of the precipitate from the control experiment The major elements of the precipitate obtained at a Ca/As molar ratio of 2.0:1, a liquid/solid mass ratio 4.0:1 and a temperature of 25°C for 5 h are shown in Table 1:

PT

Ca 37.9%, O 32.5%, As 23.7 and Na 5.75. The characterization of the control sample

RI

is presented in Fig. 2. As shown in Fig. 2a and 2b, the general particles are in irregular

SC

shapes, and no obvious crystal structure is presented. The amorphous particles

NU

agglomerate into large particles. EDS results show the control sample is mainly composed of Ca and As, indicating that the amorphous particles are Ca-As

MA

compounds. Fig. 2c shows a wide range of particle size distribution from 0.2 μm to 70 μm. The size of the particles is distributed in three concentrated areas approximately

PT E

D

0.54 μm, 4.66 μm and 19.3 μm. The median particle size (D50) of 15.5 μm reflects indirectly that most small particles are agglomerated into large particles. Fig. 2d

CE

shows that the characteristic diffraction peaks of Ca(OH)2 (portlandite), CaHAsO4·2H2O (pharmacolite) and Ca5(AsO4)3OH (johnbaumite) are observed in the

AC

control sample. A leaching test was performed using the TCLP method, and the results indicated that the arsenic-leachate concentration was 28.26 mg/L, which is greater than the regulation limit of 5 mg/L for As.

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

MA

NU

SC

RI

PT

Table 1. Chemical compositions of control sample obtained using XRF (mass fraction, %) Element Ca O As Na Percentage 37.9 32.5 23.7 5.75

MA

NU

SC

RI

PT

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

Fig. 2. Characterization of the control sample: (a) SEM, (b) EDS, (c) Particle size distribution, and (d) X-ray diffraction pattern.

ACCEPTED MANUSCRIPT

3.2. Chemical composition of precipitates The elemental composition of precipitates, obtained by crystallization reaction with different anions, was determined using XRF, and the results are shown in Fig. 3. It shows that there are no obvious changes in chemical composition in the Cl- and SO42-

PT

samples, while CO32- caused a significant change. As shown in Fig. 3a and Fig. 3b,

RI

the percentages of arsenic presented in the residuals are approximately 24% and 23%,

SC

respectively. With an increase in anion concentration, the content of Cl and S

NU

increased slightly, indicating that a portion of Cl- and SO42- entered into precipitates during the calcium-arsenate crystallization process. However, as shown in Fig. 3 c,

MA

with the increasing CO32- concentration from 0.1 mol/L to 1.0 mol/L, the content of As in the precipitates decreased from 23.7% to 11.7%, and the content of Ca

PT E

D

decreased from 34.6% to 22.2%. At the same time, the content of Na and O increased relatively. The results indicate that Cl- and SO42- can maintain As in residual and show

CE

an insignificant effect on the content of Ca-As compounds in precipitates. However, the increase in CO32- hinders the formation of Ca-As compounds and leads to arsenic

AC

release into solution.

PT

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

MA

NU

SC

RI

Fig. 3. Elemental composition of precipitates obtained by crystallization reaction with different anions: (a) chloride, (b) sulfate and (c) carbonate.

ACCEPTED MANUSCRIPT

3.3. Effect of anions on Ca-As compound crystalline structure and arsenic stability 3.3.1. Effects of Cl- concentration To investigate the influence of anions on the phase composition and crystal

PT

structure of the precipitates, a crystallization reaction was performed at 25°C for 5 h

RI

with a Ca/As molar ratio of 2.0, maintaining the anion concentration within the range

SC

of 0.1–1.0 mol/L. The XRD patterns and grain sizes of the samples synthesized at

NU

different NaCl concentrations are presented in Fig. 4. Fig. 4a shows that the characteristic diffraction peaks of Ca(OH)2, CaHAsO4·2H2O and Ca5(AsO4)3OH are

MA

observed when the Cl- concentration is 0.1 mol/L. This is similar to that of the control sample. The main reactions are shown in from Eq. 2 to Eq. 4. However, when the Cl-

PT E

D

concentration increases from 0.3 mol/L to 1.0 mol/L, CaHAsO4·2H2O diffraction peaks disappear, while Ca5(AsO4)3Cl (turneaureite) diffraction peaks become stronger,

CE

validating the formation and growth of stable calcium arsenate apatite crystals (including johnbaumite and turneaureite). The grain size was calculated using

AC

Scherrer’s equation and the results are shown in Fig. 4b. It can be seen that the grain size increased gradually with the increase in Cl- concentration. The results indicate that a low concentration of chloride shows no obvious influence on the crystallization reaction, but a high concentration of chloride can accelerate the formation and growth of calcium arsenate apatite in the form of Ca5(AsO4)3OH and Ca5(AsO4)3Cl. 𝐶𝑎(𝑂𝐻)2 + 𝑁𝑎3 𝐴𝑠𝑂4 ∙ 12𝐻2𝑂

CaH𝐴𝑠𝑂4 ∙ 2𝐻2 𝑂 + 3𝑁𝑎𝑂𝐻 + 9𝐻2 𝑂

(2)

ACCEPTED MANUSCRIPT 5𝐶𝑎(𝑂𝐻)2 + 3𝑁𝑎3 𝐴𝑠𝑂4 ∙ 12𝐻2𝑂

𝐶𝑎5 (𝐴𝑠𝑂4 )3 𝑂𝐻 + 9𝑁𝑎𝑂𝐻 + 12𝐻2 𝑂

5𝐶𝑎(𝑂𝐻)2 + 3𝑁𝑎3 𝐴𝑠𝑂4 ∙ 12𝐻2𝑂 + 𝑁𝑎𝐶𝑙

𝐶𝑎5(𝐴𝑠𝑂4 )3 𝐶𝑙 + 10𝑁𝑎𝑂𝐻 + 12𝐻2 𝑂

(3) (4)

Fig. 4b shows the effect of Cl- concentration on arsenic-leachate concentration using the TCLP test. It can be seen that the arsenic-leachate concentration decreased

PT

from 28.26 mg/L to 0.08 mg/L gradually as the Cl- concentration increased from 0

RI

mol/L to 1.0 mol/L. When Cl- concentration increased to 0.8 mol/L, the

SC

arsenic-leachate concentration reached the regulatory level (less than 5 mg/L).

NU

Meanwhile, the grain size of the calcium arsenate crystal increases gradually along with the Cl- concentration, which is opposite to the trend of the arsenic-leachate

MA

concentration. The results indicate that a larger-size calcium arsenate crystal particle is more stable than a smaller one, and chloride ion can promote an increase in the size

PT E

D

of the calcium arsenate crystals. When a chloride ion exists, the calcium arsenate crystallization reaction will move in the direction of Eq. 3 and generate Ca5(AsO4)3Cl

CE

under certain conditions. At the same time, the reaction of Eq. 2 will also be promoted, because Ca5(AsO4)3OH has similar structure and properties as compared to

AC

Ca5(AsO4)3Cl (Biagioni et al., 2017). The chloride ion potentially acts as a precursor in the formation of Ca5(AsO4)3OH and Ca5(AsO4)3Cl.

PT

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

MA

NU

SC

RI

Fig. 4. The XRD pattern (a), arsenic-leachate concentration and grain size (b) of Ca-As compounds obtained by crystallization reaction with different Clconcentrations.

ACCEPTED MANUSCRIPT 3.3.2. Effects of SO42- concentration Fig. 5a shows that the characteristic diffraction peaks of Ca4(OH)2(AsO4)2·4H2O (calcium arsenate hydroxide hydrate) and Ca(OH)2 were observed in the patterns of samples under an SO42- concentration less than 0.3 mol/L or greater than 0.8 mol/L.

PT

The diffraction peak intensity of Ca4(OH)2(AsO4)2·4H2O initially decreased and then

RI

increased when the SO42- concentration increased form 0.1 mol/L to 1.0 mol/L. In

SC

particular, the Ca4(OH)2(AsO4)2·4H2O diffraction peaks disappeared and were

NU

replaced by Ca5(AsO4)3OH and NaCaAsO4·3H2O (sodium calcium arsenate hydrate) under 0.5 mol/L SO42- concentration. The results indicate that sulfate addition mainly

MA

resulted in the formation of Ca4(OH)2(AsO4)2·4H2O (Eq. 5). However, Ca5(AsO4)3OH and NaCaAsO4·3H2O were generated when the SO42- concentration was near 0.5

PT E

D

mol/L (Eqs. 3 and 6). Actually, the sulfate ion will react with calcium and produce CaSO4 (Eq. 7), which will also participate in the calcium-arsenate crystallization

CE

reaction and promote the formation of Ca4(OH)2(AsO4)2·4H2O (Eq. 8). Although calcium sulfate was produced and then take part in another reaction immediately, this

AC

process and behavior might be vital to the formation of Ca4(OH)2(AsO4)2·4H2O. 4𝐶𝑎(𝑂𝐻)2 + 2𝑁𝑎3 𝐴𝑠𝑂4 ∙ 12𝐻2𝑂 𝐶𝑎(𝑂𝐻)2 + 𝑁𝑎3 𝐴𝑠𝑂4 ∙ 12𝐻2𝑂 Ca( H)2 + 𝑁𝑎2 𝑂4

𝐶𝑎4 (𝑂𝐻)2 (𝐴𝑠𝑂4 )2 ∙ 4𝐻2 𝑂 + 6𝑁𝑎𝑂𝐻 + 20𝐻2 𝑂 NaCa𝐴𝑠𝑂4 ∙ 3𝐻2 𝑂 + 2𝑁𝑎𝑂𝐻 + 9𝐻2 𝑂

𝐶𝑎 𝑂4 + 2𝑁𝑎 H

3Ca( H)2 + 2𝑁𝑎3 𝐴𝑠𝑂4 ∙ 12𝐻2 𝑂 + 𝐶𝑎 𝑂4 𝑁𝑎2 𝑂4 + 20𝐻2 𝑂

(5) (6) (7)

𝐶𝑎4(𝑂𝐻)2 (𝐴𝑠𝑂4 )2 ∙ 4𝐻2 𝑂 + 4𝑁𝑎 H + (8)

ACCEPTED MANUSCRIPT

The effect of sulfate on grain size and arsenic stability is also shown in Fig. 5b. When the SO42- concentration is 0.1 mol/L, the arsenic-leachate concentration is 2.75 mg/L, which is lower than that of the control sample (28.26 mg/L) and meets the standard level (less than 5 mg/L). Thus, sulfate is beneficial in reducing the

PT

arsenic-leachate concentration from Ca-As precipitates. Along with an SO42-

RI

concentration increase from 0.1 mol/L to 1.0 mol/L, arsenic-leachate concentration

SC

initially increased to 10.17 mg/L and then decreased to 3.75 mg/L. Combined with

NU

XRD results, the generation of stable Ca4(OH)2(AsO4)2·4H2O crystals should be the main reason for the reduction in the arsenic-leachate concentration. The trend of grain

MA

size was opposite to that of arsenic-leachate concentration, further illustrating that larger Ca4(OH)2(AsO4)2·4H2O crystals are more stable. However, Ca5(AsO4)3OH and

PT E

D

NaCaAsO4·3H2O were generated when the SO42- concentration was near 0.5 mol/L. Perhaps NaCaAsO4·3H2O is not very stable compared to Ca5(AsO4)3OH and

CE

Ca4(OH)2(AsO4)2·4H2O and that is the reason the arsenic-leachate concentration

AC

increased during the TCLP test.

PT

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

MA

NU

SC

RI

Fig. 5. The XRD pattern (a), arsenic-leachate concentration and grain size (b) of Ca-As compounds obtained by crystallization reaction with different SO42concentrations.

ACCEPTED MANUSCRIPT 3.3.3. Effects of CO32- concentration The XRD patterns of the samples under different CO32- concentrations are presented in Fig. 6a. The patterns show that compared to the control sample, the characteristic diffraction peaks of Ca4(OH)2(AsO4)2·4H2O instead of Ca5(AsO4)3OH

PT

were generated when the carbonate concentration is 0.1 mol/L. When CO32-

RI

concentration increased from 0.3 to 1.0 mol/L, the phase composition of the

SC

precipitates is different from one another. There are no calcium-arsenic compounds

NU

formed except Ca4(OH)2(AsO4)2·4H2O under a CO32- concentration less than 0.3 mol/L. With increasing carbonate concentrations, CaCO3 (calcite), Na3AsO4 (sodium

MA

arsenate), Na3AsO4·12H2O (sodium arsenate hydrate), and Na3Ca(CO3)2·5H2O (gaylussite) were generated successively. The results indicate that a low carbonate

PT E

D

concentration would not be disadvantageous for arsenic-leachate concentrations but would promote the crystallization of Ca4(OH)2(AsO4)2·4H2O. However, a higher

CE

carbonate concentration might inhibit the reaction between AsO43- and Ca2+ and produce calcium-carbonate compounds.

AC

The effect of carbonate on grain size and arsenic stability under a CO32concentration from 0 mol/L to 1.0 mol/L is presented in Fig. 6b. It can be seen that the arsenic-leachate concentration initially decreased from 28.26 mg/L to 18.66 mg/L and then increased dramatically to 1412.50 mg/L after the CO32- concentration exceeded 0.5 mol/L. However, the lowest arsenic-leachate concentration of precipitates under the function of carbonate was still higher than the threshold value of the TCLP

ACCEPTED MANUSCRIPT

standard level. Because there are no Ca-As compound crystals generated under a high CO32- concentration, the grain size of precipitates is not valuable for arsenic-leachate concentration. Under a low concentration of carbonate, calcium arsenates can normally be generated mainly because of the excessive calcium, and the carbonate

PT

reacts with the excessive calcium ion first. Therefore, a low concentration of

RI

carbonate shows no obvious influence on the crystallization of Ca-As compounds.

SC

However, when the carbonate concentration continues to increase, it will compete for

NU

calcium ions and prevent the formation of calcium arsenates. The diffraction peak of

AC

CE

PT E

D

grain size could not be calculated.

MA

the Ca-As compounds in the XRD pattern correspondingly disappeared, such that the

PT

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

MA

NU

SC

RI

Fig. 6. The XRD pattern (a), arsenic-leachate concentration and grain size (b) of Ca-As compounds obtained by crystallization reactions with different CO32concentrations.

ACCEPTED MANUSCRIPT

3.4. Effect of anions on morphological features Morphological features play an important role in the structure and stability of Ca-As compounds (Zhu et al., 2006). The morphology of the precipitates identified by XRD was examined systematically using SEM-EDS and the results are shown in Fig.

PT

7 and Fig. 8. The particle size distribution of these samples is provided in Fig. 9. As

RI

observed in Fig. 7, the anions have a significant influence on the crystal structure of

SC

the precipitates. Fig. 7a–d is the SEM micrograph of the Ca-As compounds under a

NU

different Cl- concentration treatment. It can be seen from the pictures that the particles of the Ca-As compounds become more compact and smooth with increasing Cl-

MA

concentration. The particle size distribution curve in Fig. 9a shows that these precipitates share nearly the same particle size distribution and median diameter (D50).

PT E

D

As shown in Fig. 9d, the median diameters are 16.8 μm, 18.7 μm and 18.8 μm, which are close to that of the control sample (15.5 μm). Compared to the SEM image of the

CE

control sample in a large agglomerated particle (Fig. 2a), Fig. 7a is mainly for capturing the small amorphous particles. The EDS results from Fig. 8a and Fig. 2b

AC

show that the chemical composition of particle A as shown in Fig. 7a is different from that of the control sample. The content of Ca and As shown in Fig. 7a is 29.0% and 37.2%, while that shown in Fig. 2a is 33.8% and 21.0%, respectively. The Ca/As ratio of particle A is much lower than that of the control sample. Combined with the results of XRD, the amorphous particles in Fig. 7a might be CaHAsO4·2H2O, while the agglomerated particle in Fig. 2a might be Ca5(AsO4)3OH. Fig. 7d shows rod-shaped

ACCEPTED MANUSCRIPT particles were formed under the condition of a 1.0-mol/L Cl- concentration treatment. The EDS spectra focused on the area in Fig. 7c shows that Cl was present in the particle. Combined with the XRD patterns, these rod-shaped particles are Ca5(AsO4)3OH and Ca5(AsO4)3Cl. This result supports the conclusion that increasing

PT

chloride promotes the formation and growth of calcium arsenate apatite crystals, the

RI

structure of which is more stable than the amorphous calcium arsenates (Biagioni et

SC

al., 2017; Biagioni and Pasero, 2013), thus leading to a low arsenic-leachate

NU

concentration.

SEM microphotographs of the samples affected by different SO42- concentrations

MA

are shown in Fig. 7e–h. Based on these microphotographs, it can be seen that strip crystals 3–5 μm in length were observed under the SO42- at less than 0.3 mol/L or

PT E

D

greater than 0.8 mol/L. The EDS spectra (Fig. 8d and f) show that the micro-area elements at point D and point F in the strip crystals are Ca, Na, O and As. Combined

CE

with the XRD results, these crystals are Ca4(OH)2(AsO4)2·4H2O. However, the microstructure is not in an obvious crystal-shape at an SO42- concentration of 0.5

AC

mol/L (Fig. 7f). Thus, the calcium arsenate crystals are rarely formed in the crystallization system with a 0.5-mol/L sulfate addition. Combined with the XRD pattern (Fig. 5a) and EDS diagram (Fig. 8e), the poorly crystallized particles are probably NaCaAsO4·3H2O, thus leading to more arsenic leaching out during the TCLP test, which corresponds with the results of other studies (Yoon et al., 2010). The particle size distribution shown in Fig. 9b also demonstrates that the main

ACCEPTED MANUSCRIPT

distribution areas of particles under the 0.5-mol/L sulfate treatment are smaller than the particles under the 0.1-mol/L or 1.0-mol/L sulfate treatments. The results indicate that low or high sulfate will lead to calcium arsenate crystal form transformation and densification, which will increase its crystallinity and stability.

PT

The SEM micrographs of samples of different CO32- concentration treatments are

RI

presented in Fig. 7i–m. Fig. 7i shows that a longer and larger strip crystal with a

SC

length of from 10–15 μm was observed when the CO32- concentration was 0.1 mol/L.

NU

The EDS spectra (Fig. 8g) combined with the XRD patterns (Fig. 6a) illustrate that the strip crystal is Ca4(OH)2(AsO4)2·4H2O. Fig. 9c shows that the particle size

MA

distribution of this Ca-As compound is relatively larger than that of the others, having a larger median diameter of 26.5 μm. However, the strip crystal became incomplete

PT E

D

and released amorphous particles gradually along with the increasing CO32concentration (Fig. 7j and 7k), causing the size of the particles to decrease. This may

CE

be a result of the Ca2+ and Na+ reacting with carbonate and generating CaCO3 or Na3Ca(CO3)2·5H2O, which would lead to arsenic emission to aqueous solution (Zhu

AC

et al., 2006). When CO32- the concentration is 0.8 mol/L, the SEM image shows particles tend to aggregate in a flocculent structure (Fig. 7k). The EDS spectra (Fig. 8h) shows the microregion elemental distribution contains Ca, O, Na and As. Combined with XRD patterns, this finding indicates that the flocculent structure is Na3AsO4·12H2O within in a matrix of calcium hydroxide. A shown in Fig. 7l, bulk crystals were observed when the CO32- concentration reached 1.0 mol/L. The EDS

ACCEPTED MANUSCRIPT

spectra (Fig. 8i) showed the existence of Ca, Na and C, illustrating that the bulk crystal

is

Na3Ca(CO3)2·5H2O.

Therefore,

during

the

treatment

of

some

arsenic-containing wastes with high carbonate ion concentration, such as high alkaline arsenic-bearing sludges in antimony smelting, the formation of calcium arsenate

PT

crystals may be affected. Excessive carbonate should be avoided as much as possible

RI

in the treatment of arsenic-containing wastewater or arsenic-bearing sludges based on

AC

CE

PT E

D

MA

NU

SC

calcium arsenate crystallization.

NU

SC

RI

PT

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

MA

Fig. 7. SEM images of Ca-As compounds with different anion concentrations.

MA

NU

SC

RI

PT

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

Fig. 8. EDS plots of Ca-As compounds with different anion concentrations.

RI

PT

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

MA

NU

SC

Fig. 9. Particle size distribution of precipitates obtained by crystallization reaction with different anions: (a) chloride, (b) sulfate and (c) carbonate, and the variation in the cumulative size distribution: (d) chloride, (e) sulfate and (f) carbonate.

ACCEPTED MANUSCRIPT

Typical bright-field TEM and high-resolution transmission electron microscopy (HRTEM) were employed to investigate the internal structure of the as-prepared Ca-As compounds. As shown in Fig. 10a and 10d, it can be seen that the particle size is at a nanometre scale, and the crystals are randomly distributed under a 1.0-mol/L

PT

Cl- concentration influence. Combined with the XRD and SEM results, these crystals

RI

might be Ca5(AsO4)3OH and Ca5(AsO4)3Cl. The TEM micrographs and the HRTEM

SC

images of Ca4(OH)2(AsO4)2·4H2O affected by 1.0 mol/L SO42- and 0.1 mol/L CO32-

NU

are shown in Fig. 10b and 10e and Fig. 10c and 10f, respectively. It can be seen that the μm-scale particle is Ca4(OH)2(AsO4)2·4H2O, corresponding with the strip crystal

MA

shown in the previously mentioned SEM micrograph (Fig. 7h and 7i). The HRTEM images show that the diffraction fringes are consistent with lattice fringes, illustrating

PT E

D

the crystalline grains are nanoparticles. The results also indicate that the internal structure of the Ca4(OH)2(AsO4)2·4H2O crystals is affected by different anions, and

AC

CE

the structure is quite distinguishable.

RI

PT

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

MA

NU

SC

Fig. 10. TEM and HR-TEM images of Ca-As compounds. (a)TEM and (d) HR-TEM images of calcium arsenate apatite with 1.0-mol/L Cl- addition, (b)TEM and (e) HR-TEM images of Ca4(OH)2(AsO4)2·4H2O with 1.0-mol/L SO42- addition, (c)TEM and (f) HR-TEM images of Ca4(OH)2(AsO4)2·4H2O with 0.1-mol/L CO32- addition.

ACCEPTED MANUSCRIPT

4. Conclusion The calcium arsenate crystallization reaction can be affected by common anions, such as chloride, sulfate and carbonate. Chloride and sulfate show an insignificant effect on the content of Ca-As compounds in precipitates, while carbonate results in a

PT

decrease in Ca-As compounds. The anions have an effect on the arsenic-leachate

RI

concentration which is related to the grain size of the calcium arsenate crystals.

SC

Chloride can contribute to the crystallization reaction and promote the formation and

NU

growth of arsenic apatite, which can effectively reduce the arsenic-leachate concentration of the precipitates. When the Cl- concentration increased from 0 mol/L

MA

to 1.0 mol/L, the arsenic-leachate concentration decreased from 28.26 mg/L to 0.08 mg/L. The chloride ion potentially acts as a precursor in the formation and growth of

PT E

D

Ca5(AsO4)3OH and Ca5(AsO4)3Cl crystals, resulting in the arsenic-leachate concentration gradually decreasing. Sulfate is beneficial in reducing the

CE

arsenic-leachate concentration from Ca-As precipitates, because it is propitious to improve the formation and growth of Ca4(OH)2(AsO4)2·4H2O. Low or high sulfate

AC

will lead to calcium arsenate crystal form transformation and densification, which will increase its crystallinity and stability. A low carbonate concentration does not have a detrimental effect on the arsenic-leachate concentration in the short term. In contrast, a small amount of carbonate is beneficial for the formation and growth of Ca4(OH)2(AsO4)2·4H2O. However, more carbonate would capture Ca2+ and Na+ to generate CaCO3 and Na3Ca(CO3)2·5H2O instead of Ca-As compounds, which would

ACCEPTED MANUSCRIPT

prevent the calcium arsenate crystallization reaction. The trend of grain size being in opposition to that of the arsenic-leachate concentration illustrates that the larger crystal particles of Ca-As compounds are more stable than the smaller ones. Thus, promoting grain size growth of stable calcium

PT

arsenates by controlling the anion concentration to reduce the arsenic-leachate

RI

concentration is a proposed method for industrial applications.

SC

Acknowledgements

NU

This work was supported by the Special Program on Environmental Protection for Public Welfare (201509050), the National Natural Science Foundation of China

MA

(51704337, 51474247, 51634010), the National Key R&D Program of China (2017YFC0210402), and the Co-Innovation Center for Clean and Efficient Utilization

AC

CE

PT E

D

of Strategic Metal Mineral Resources for financial support.

ACCEPTED MANUSCRIPT

References

AC

CE

PT E

D

MA

NU

SC

RI

PT

Biagioni, C., Bosi, F., Hålenius, U. and Pasero, M., 2017. The crystal structure of turneaureite, Ca5(AsO4)3Cl, the arsenate analogue of chlorapatite, and its relationships with the arsenate apatites johnbaumite and svabite. Am. Mineral., 102. DOI: http://dx.doi.org/10.2138/am-2017-6041. Biagioni, C. and Pasero, M., 2013. The crystal structure of johnbaumite, Ca5(AsO4)3OH, the arsenate analogue of hydroxylapatite. Am. Mineral., 98(8-9): 1580-1584. Bothe, J.V. and Brown, P.W., 1999. Arsenic immobilization by calcium arsenate formation. Environ. Sci. Technol., 33(21): 3806-3811. Camacho, J., Wee, H.Y., Kramer, T.A. and Autenrieth, R., 2009. Arsenic stabilization on water treatment residuals by calcium addition. J. Hazard. Mater., 165(1-3): 599-603. Chai, L.Y., Yang, J.Q., Zhang, N., Wu, P.J., Li, Q.Z., Wang, Q.W., Liu, H. and Yi, H.B. 2017. Structure and spectroscopic study of aqueous Fe(III)-As(V) complexes using UV-Vis, XAS and DFT-TDDFT. Chemosphere, 182: 595-604. Chen, Y.P., Dong, H., Zeng, Q.R., Song, H.J., Chai, L.Y. and Gu, J.D., 2015. Removal of Trace As(V) from Water with the Titanium Dioxide/ACF Composite Electrode. Water Air Soil Pollut., 226(7). Choi, W.H., Lee, S.R. and Park, J.Y., 2009. Cement based solidification/stabilization of arsenic-contaminated mine tailings. Waste Manag., 29(5): 1766-1771. Crundwell, F.K., 2016. A novel mechanism for the rate of growth during the crystallisation of salts and the precipitation of minerals. Hydrometallurgy, 166: 62-72. Cui, J., Du, Y.G., Xiao, H.X., Yi, Q.S. and Du, D.Y., 2014. A new process of continuous three-stage co-precipitation of arsenic with ferrous iron and lime. Hydrometallurgy, 146: 169-174. Donahue, R. and Hendry, M.J., 2003. Geochemistry of arsenic in uranium mine mill tailings, Saskatchewan, Canada. Appl. Geochem., 18(11): 1733-1750. Fei, J.C., Min, X.B., Wang, Z.X., Pang, Z.H., Liang, Y.J. and Ke, Y., 2017. Health and ecological risk assessment of heavy metals pollution in an antimony mining region: a case study from South China. Environ. Sci. Pollut. Res., DOI : 10.1007/s11356-017-0310-x. Ke, Y., Min, X.B., Chai, L.Y., Zhou, B.S. and Xue, K., 2016. Sulfidation behavior of Zn and ZnS crystal growth kinetics for Zn(OH)2-S-NaOH hydrothermal system. Hydrometallurgy, 161: 166-173. Kontrec, J. Kralj, D., Brecevic, L., Falini, G., Fermani, S., Noethig-Laslo, V. and Mirosavljevic, K., 2004. Incorporation of inorganic anions in calcite. Eur. J. Inorg. Chem.(23): 4579-4585.

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

MA

NU

SC

RI

PT

Lei, J., Peng, B., Min, X. B., Liang, Y. J., You, Y. and Chai, L. Y., 2017. Modeling and optimization of lime-based stabilization in high alkaline arsenic-bearing sludges with a central composite design. J. Environ. Sci. Health A Tox. Hazard Subst. Environ. Eng., 52(5): 449-458. Li, Y.C., Min, X. B., Chai, L. Y., Shi, M. Q., Tang, C. J., Wang, Q. W., Liang, Y. J., Lei, J. and Liyang, W. J., 2016. Co-treatment of gypsum sludge and Pb/Zn smelting slag for the solidification of sludge containing arsenic and heavy metals. J. Environ. Manag., 181: 756-761. Li, Y.C., Min, X.B., Ke, Y., Chai, L.Y., Shi, M.Q., Tang, C.J., Wang, Q.W., Liang, Y.J., Lei, J. and Liu, D.G., 2017. Utilization of red mud and Pb/Zn smelter waste for the synthesis of a red mud-based cementitious material. J. Hazard. Mater. DOI: 10.1016/j.jhazmat.2017.10.046 Li, Y.H., Liu, Z. H., Li, Q. H., Zhao, Z. W., Liu, Z. Y., Zeng, L. and Li, L., 2011. Removal of arsenic from arsenate complex contained in secondary zinc oxide. Hydrometallurgy, 109(3-4): 237-244. Li, Y.R., Wang, J., Peng, X.J., Ni, F. and Luan, Z.K., 2012. Evaluation of arsenic immobilization in red mud by CO2 or waste acid acidification combined ferrous (Fe2+) treatment. J. Hazard. Mater., 199: 43-50. Liang, Y.J., Min, X. B., Chai, L. Y., Wang, M., Liyang, W. J., Pan, Q. L. and Okido, M., 2017. Stabilization of arsenic sludge with mechanochemically modified zero valent iron. Chemosphere, 168: 1142-1151. Liu, D.G., Min, X.B., Ke, Y., Chai, L.Y., Liang, Y.J., Li, Y.C., Yao, L.W. and Wang, Z.B., 2017. Co-treatment of flotation waste, neutralization sludge, and arsenic-containing gypsum sludge from copper smelting: solidification/stabilization of arsenic and heavy metals with minimal cement clinker. Environ. Sci. Pollut. Res., DOI: 10.1007/s11356-017-1084-x Luo, T., Cui, J.L., Hu, S., Huang, Y.Y. and Jing, C.Y., 2010. Arsenic Removal and Recovery from Copper Smelting Wastewater Using TiO2. Environ. Sci. Technol., 44(23): 9094-9098. Meng, X.G., Korfiatis, G.P., Bang, S.B. and Bang, K.W., 2002. Combined effects of anions on arsenic removal by iron hydroxides. Toxicol. Lett., 133(1): 103-111. Min, X.B., Li, Y. W. J., Ke, Y., Shi, M. Q., Chai, L. Y. and Xue, K., 2017. Fe-FeS2 adsorbent preparedwith ironpowder and pyrite by facile ball milling and its application for arsenic removal. Water Sci. Technol., 76(1): 192-200. Min, X.B., Yuan, C. Y., Chai, L. Y., Liang, Y. J., Zhang, H. J., Xie, X. D. and Ke, Y., 2013. Hydrothermal modification to improve the floatability of ZnS crystals. Miner. Eng., 40: 16-23. Morales, A., Cruells, M., Roca, A. and Bergo, R., 2010. Treatment of copper flash smelter flue dusts for copper and zinc extraction and arsenic stabilization. Hydrometallurgy, 105(1-2): 148-154.

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

MA

NU

SC

RI

PT

Ozverdl, A. and Erdem, M., 2010. Environmental risk assessment and stabilization/solidification of zinc extraction residue: I. Environmental risk assessment. Hydrometallurgy, 100(3-4): 103-109. Peng, C., Chai, L.Y., Tang, C.J., Min, X.B., Song, Y.X., Duan, C.S. and Yu, C., 2017. Study on the mechanism of copper-ammonia complex decomposition in struvite formation process and enhanced ammonia and copper removal. J. Environ. Sci., 51: 222-233. Petrik, L., 2009. The influence of cation, anion and water content on the rate of formation and pore size distribution of zeolite ZSM-5. S. Afr. J. Sci., 105(7-8): 251-257. Randall, P.M., 2012. Arsenic encapsulation using Portland cement with ferrous sulfate/lime and Terra-Bond (TM) technologies - Microcharacterization and leaching studies. Sci. Total Environ., 420: 300-312. Rivas, B.L., Pereira, E., Paredes, J. and Sanchez, J., 2012. Removal of arsenate from ionic mixture by anion exchanger water-soluble polymers combined with ultrafiltration membranes. Polym. Bull., 69(9): 1007-1022. Shaw, J.K., Fathordoobadi, S., Zelinski, B.J., Ela, W.P. and Saez, A.E., 2008. Stabilization of arsenic-bearing solid residuals in polymeric matrices. J. Hazard. Mater., 152(3): 1115-1121. Sun, Y.K., Hu, Y. H., Huang, T. L., Li, J. X., Qin, H. J. and Guan, X. H., 2017. Combined Effect of Weak Magnetic Fields and Anions on Arsenite Sequestration by Zerovalent Iron: Kinetics and Mechanisms. Environ. Sci. Technol., 51(7): 3742-3750. Tanboonchuy, V., Grisdanurak, N. and Liao, C.H., 2012. Background species effect on aqueous arsenic removal by nano zero-valent iron using fractional factorial design. J. Hazard. Mater., 205: 40-46. USEPA, 1992. Method 1311, Toxicity Characteristic Leaching Procedure. Washington DC. Vinals, J., Sunyer, A., Molera, P., Cruells, M. and Llorca, N., 2010. Arsenic stabilization of calcium arsenate waste by hydrothermal precipitation of arsenical natroalunite. Hydrometallurgy, 104(2): 247-259. Wang, Z.X., Chai, L.Y., Wang, Y.Y., Yang, Z.H., Wang, H.Y. and Wu, X., 2011. Potential health risk of arsenic and cadmium in groundwater near Xiangjiang River, China: a case study for risk assessment and management of toxic substances. Environ. Monit. Assess., 175(1-4): 167-173. Welham, N.J., Malatt, K.A. and Vukcevic, S., 2000. The effect of solution speciation on iron-sulphur-arsenic-chloride systems at 298 K. Hydrometallurgy, 57(3): 209-223. Wu, C., Zou, Q., Xue, S.G., Pan, W.S., Huang, L., Hartley, W., Mo, J.Y. and Wong, M.H., 2016. The effect of silicon on iron plaque formation and arsenic accumulation in rice genotypes with different radial oxygen loss (ROL). Environ. Pollut., 212: 27-33.

ACCEPTED MANUSCRIPT

AC

CE

PT E

D

MA

NU

SC

RI

PT

Xie, X.D., Min, X. B., Chai, L. Y., Tang, C. J., Liang, Y. J., Li, M., Ke, Y., Chen, J. and Wang, Y., 2013. Quantitative evaluation of environmental risks of flotation tailings from hydrothermal sulfidation-flotation process. Environ. Sci. Pollut. Res., 20(9): 6050-6058. Yoon, I.H., Moon, D. H., Kim, K. W., Lee, K. Y., Lee, J. H. and Kim, M. G., 2010. Mechanism for the stabilization/solidification of arsenic-contaminated soils with Portland cement and cement kiln dust. J. Environ. Manag., 91(11): 2322-2328. Zhang, R., Sun, H. and Yin, J., 2008. Arsenic and chromate removal from water by iron chips—Effects of anions. Front. Environ. Sci. Eng. Chin., 2(2): 203-208. Zhao, Z.W., Chai, L.Y., Peng, B., Liang, Y.J., He, Y.H. and Yan, Z.H., 2017. Arsenic vitrification by copper slag based glass: Mechanism and stability studies. J. Non-Cryst. Solids, 466: 21-28. Zhu, Y.N., Zhang, X.H., Xie, Q.L., Wang, D.Q. and Cheng, G.W., 2006. Solubility and stability of calcium arsenates at 25 degrees C. Water Air Soil Pollut., 169(1-4): 221-238.

ACCEPTED MANUSCRIPT

Highlights 

The anions, including chloride, sulfate and carbonate, have an effect on the calcium arsenate crystallization reaction.



Chloride and sulfate contribute to the crystallization reaction while carbonate would prevent the formation of calcium arsenate. The arsenic leachate concentration of Ca-As compounds is related to the grain

PT



size of calcium arsenate crystals.

RI

The larger crystal particles of calcium arsenate are more stable than the

CE

PT E

D

MA

NU

SC

smaller one.

AC