n-TNA ternary heterojunction electrode for tetracycline degradation

n-TNA ternary heterojunction electrode for tetracycline degradation

Accepted Manuscript Title: Photoeletrocatalytic Activity of an n-ZnO/p-Cu2 O/n-TNA Ternary Heterojunction Electrode for Tetracycline Degradation Autho...

486KB Sizes 3 Downloads 54 Views

Accepted Manuscript Title: Photoeletrocatalytic Activity of an n-ZnO/p-Cu2 O/n-TNA Ternary Heterojunction Electrode for Tetracycline Degradation Author: Jinhua Li Shubin Lv Yanbiao Liu Jing Bai Baoxue Zhou Xiaofang Hu PII: DOI: Reference:

S0304-3894(13)00646-8 http://dx.doi.org/doi:10.1016/j.jhazmat.2013.09.002 HAZMAT 15382

To appear in:

Journal of Hazardous Materials

Received date: Revised date: Accepted date:

4-7-2013 29-8-2013 3-9-2013

Please cite this article as: J. Li, S. Lv, Y. Liu, J. Bai, B. Zhou, X. Hu, Photoeletrocatalytic Activity of an n-ZnO/p-Cu2 O/n-TNA Ternary Heterojunction Electrode for Tetracycline Degradation, Journal of Hazardous Materials (2013), http://dx.doi.org/10.1016/j.jhazmat.2013.09.002 This is a PDF file of an unedited manuscript that has been accepted for publication. As a service to our customers we are providing this early version of the manuscript. The manuscript will undergo copyediting, typesetting, and review of the resulting proof before it is published in its final form. Please note that during the production process errors may be discovered which could affect the content, and all legal disclaimers that apply to the journal pertain.

1 2 3

ip t

4

Photoeletrocatalytic Activity of an n-ZnO/p-Cu2O/n-TNA Ternary Heterojunction Electrode

6

for Tetracycline Degradation

us

cr

5

7

an

8

Jinhua Li, Shubin Lv, Yanbiao Liu, Jing Bai, Baoxue Zhou, Xiaofang Hu

10

School of Environmental Science and Engineering, Shanghai Jiao Tong University No.800

11

Dongchuan Rd, Shanghai 200240, China

d

12

M

9

Corresponding author: Baoxue Zhou, Tel/Fax: +86-21-54747351;

14

E-mail: [email protected]

Ac ce p

te

13

1 Page 1 of 28

15

Photoeletrocatalytic Activity of an n-ZnO/p-Cu2O/n-TNA Ternary Heterojunction Electrode

16

for Tetracycline Degradation

17

Jinhua Li, Shubin Lv, Yanbiao Liu, Jing Bai, Baoxue Zhou*, Xiaofang Hu

19

School of Environmental Science and Engineering, Shanghai Jiao Tong University, Shanghai 200240,

20

China

cr

ip t

18

Abstract

22

In

23

(n-ZnO/p-Cu2O/n-TNA) nanophotocatalyst with a sandwich-like nanostructure was constructed and

24

applied for the photoelectrocatalytic (PEC) degradation of typical PPCPs, tetracycline (TC). The

25

ternary heterojunction n-ZnO/p-Cu2O/n-TNA was obtained by depositing Cu2O on the surface of

26

TNA via sonoelectrochemical deposition (SED) and subsequently building a layer of ZnO ontop the

27

p-Cu2O/n-TNA surface through hydrothermal synthesis. After being deposited by the Cu2O, the

28

absorption-band edge of the p-Cu2O/n-TNA was obviously red-shifted to the visible region (to

29

505nm), and the band gap was reduced from its original 3.20 eV to 2.46 eV. The band gap

30

absorption edge of the ternary n-ZnO/p-Cu2O/n-TNA is similar to that of p-Cu2O/n-TN and extends

31

the visible spectrum absorption to 510 nm, corresponding to an Eg value of about 2.43 eV. Under

32

illumination of visible light, the photocurrent density of the ternary heterojunction

33

n-ZnO/p-Cu2O/n-TNA electrode at 0.5V (vs. Ag/AgCl) was more than 106 times as high as that of

34

the pure TNAs electrode, 3.6 times as high as that of the binary heterojunction p-Cu2O/n-TNA

35

electrode. The degradation of TC indicated that the ternary heterojunction n-ZnO/p-Cu2O/n-TNA

study,

a

novel

ternary

heterojunction

n-ZnO/p-Cu2O/n-TiO2

nanotube

arrays

Ac ce p

te

d

M

an

this

us

21

Corresponding author: Baoxue Zhou, Tel/Fax: +86-21-54747351 *

Abbreviations: TC, tetracycline; CB, conduction band; VB, valence band; TNA, TiO2 nanotube arrays;.PEC, photoelectrocatalytic; SED, sonoelectrochemical deposition method

2 Page 2 of 28

electrode maintained a very high photoelectrocatalytic activity and excellent stability and reliability.

37

Such kind of ternary heterojunction electrode material has a broad application prospect not only in

38

pollution control but also in many other fields.

39

Key words: Ternary heterojunction; ZnO; Cu2O; TNA; Photoeletrocatalytic oxidation

40

1. Introduction

cr

ip t

36

Photocatalysis is a promising technique in environmental purification and solar energy

42

conversion [1]. Compared with conventional treatment processes, it has advantages of environmental

43

friendliness, energy-saving property, high efficiency and non-secondary pollution [2–6]. Thus, the

44

fabrication of a high-performance semiconductor photocatalyst is a key issue in the photocatalytic

45

technology. However, the common semiconductor materials, such as TiO2 or ZnO, can only absorb

46

UV light because of their wide band gaps [7], which greatly limit the usage of solar light.

M

an

us

41

The coupled semiconductor heterojunction is an effective method to improve their

48

photoelectrocatalytic (PEC) efficiency [8]. Due to the different energy levels between the conduction

49

bands (CB) of the semiconductors, the photoexcited electrons can be quickly passed from one

50

semiconductor to a neighboring semiconductor so as to accelerate electron-hole pair separation and

51

improve PEC efficiency.

Ac ce p

te

d

47

52

In the past several years, the coupling of n-ZnO or n-TiO2 with other metal oxides or sulfides

53

such as, n-WO3, n-CdS, n-Fe2O3, p-SnO2, p-Cu2O and so on, have been reported [9–17]. Cuprous

54

oxide, Cu2O, is an attractive p-type oxide for photoelectrochemical hydrogen production with a

55

direct band gap of 2.0 eV and a light-to-hydrogen conversion efficiency of 18% based on the AM 1.5

56

spectrums [10, 18-20]. In recent years, some researchers reported the binary p-n heterojunctions by

57

coupling of p-Cu2O with n-TiO2 or n-ZnO [20-25]. In these work, an enhancement of the charge 3 Page 3 of 28

separation was achieved since the CB of Cu2O (-1.16V) is narrow than that of TiO2 (-0.1V) or ZnO

59

(-0.2V). For example, Bessekhouad et al [20] observed the Cu2O/TiO2 composite oxides via the

60

mixture of Cu2O (particle size < 5nm) with commercial P25 TiO2 exhibited a superior activity for the

61

degradation of Orange II under visible irradiation. Xu et al [21] prepared the ZnO/Cu2O compound

62

photocatalysts by “soak-deoxidize-airoxidation” and found that the photocatalytic properties of

63

ZnO/Cu2O compound were improved greatly compared with pure ZnO. When the ZnO/Cu2O

64

compound was used as photocatalyst, the degradation of MO reached 73% after 180 min of reaction.

65

In spite of some advantages by coupling Cu2O with TiO2 or ZnO, The main drawback for the use of

66

Cu2O as a photocathode is its poor stability in aqueous solutions, because the redox potentials for the

67

reduction and oxidation of monovalent copper oxide lie within the band gap [22-25]. Thus, how to

68

protect the photocatalyst Cu2O against photocorrosion is an interesting issue.

M

an

us

cr

ip t

58

Based on the above analysis and our previous work, a novel ternary heterojunction

70

n-ZnO/p-Cu2O/n-TNA photocatalyst with a sandwich-like nanostructure is proposed. The ternary

71

heterojunction n-ZnO/p-Cu2O/n-TNA material has the following advantage: first, the CB of p-Cu2O

72

is more negative than that of n-ZnO and n-TiO2, which favors the charge separation and transfer.

73

Second, the TNA as the substrate of ternary heterojunction is already a very good photocatalyst and

74

can maintain the high PEC activity in the UV region. Third, the coupling of the high PEC active

75

TNA with Cu2O having narrow band gap extends the visible spectrum absorption and favors the

76

charge separation and transfer. Fourth, the coupling of n-ZnO with binary heterojunction

77

p-Cu2O/n-TNA protects the Cu2O from photocorrosion and exhibits desirable stability.

Ac ce p

te

d

69

78

Herein, the n-ZnO/p-Cu2O/n-TNA was prepared by depositing Cu2O on the TNAs via SED and

79

then building a layer of n-ZnO on the p-Cu2O/n-TNA surface through hydrothermal synthesis. The 4 Page 4 of 28

detailed synthesis process, characterization, and photoelectrochemical property testing for this

81

composite catalyst were also discussed. In addition, the n-ZnO/p-Cu2O/n-TNA electrode was applied

82

for the degradation of PPCPs TC to evaluate the PEC performance. TC is widely used in aquiculture

83

and live stocking, but the waste TC is usually discharged along with waste water, which causes

84

serious ecological pollution.

85

2. Experimental

86

2.1. Materials

us

cr

ip t

80

Pieces of titanium (Ti) sheets (purity > 99.99%) were obtained from Kurumi works, Japan. TC

88

(C22H24N2O8·HCl), hydrofluoric acid, sodium sulfate, sodium hydroxide, and acetone were

89

purchased obtained from Shanghai Chemical Reagent Company (China) without further purification.

90

All solutions were prepared with doubly distilled deionized water.

91

2.2 The preparation of electrodes

92

2.2.1 Preparation of TNA

te

d

M

an

87

TNA was synthesized via the anodization of pretreated Ti in 0.5 % HF aqueous (HF-H2O) [24].

94

Electrochemical setup consisted of a two-electrode configuration with a platinum foil as the cathode

95

and a DC power supply (Tradex, MPS 305) was used to drive the anodization. After anodization at

96

20V for 30 min at room temperature, the as-prepared TNA samples were crystallized by annealing in

97

air atmosphere for 3 h at 450 °C with heating and cooling rates of 1º/min.

98

2.2.2 Preparation of p-Cu2O/n-TNA

Ac ce p

93

99

The p-Cu2O/n-TNA was prepared by the sonoelectrochemical deposition method (SED) [22].

100

The electrolyte solution contained 0.1 M sodium acetate and 0.02 M cupric acetate. The TNA worked

101

as the work electrode, a platinum foil was counter electrode and a saturated Ag/AgCl was reference 5 Page 5 of 28

electrode. After the deposition at -2.5v for 30 min, the samples were immediately removed from the

103

electrolyte and then rinsed with DI water. The prepared p-Cu2O/n-TNA electrodes were annealed at

104

200 °C for 60 min in nitrogen atmosphere.

105

2.2.3 Preparation of n-ZnO/p-Cu2O/n-TNA

ip t

102

The n-ZnO/p-Cu2O/n-TNA was synthesized by the hydrothermal method. First, the 0.15 M ZnO

107

coating precursor solution was prepared by dissolving 5 mM Zn(CH3COO)2 to ethanol and stirring

108

for 0.5 h. And then the precursor solution were added to the p-Cu2O/n-TNA substrate, spun at 100

109

rpm for 3 s, and then spun at 3000 rpm for 10 s. Such a cycle was repeated 5 times. Then the

110

substrate were immersed into the 0.02 M Zn (NO3)2 and (CH2)6N4 growing precursor solution at

111

90 °C for a certain time. Finally, the resultant films were washed with deionized water to remove any

112

residual materials and dried at room temperature.

113

2.3 The characteristics of electrodes

te

d

M

an

us

cr

106

The phase of products was identified by X-ray powder diffraction (XRD, Shimadzu), using Cu

115

KR (λ>0.15406 nm) radiation at 50 kV and 50 mA at a scanning rate of 8°/min in the 2θ range from

116

10 to 60° at room temperature. TEM images were collected by using a field emission scanning

117

electron microscopy (FESEM FEI-Sirion200). UV–visible absorption spectra of the samples were

118

recorded on a photospectrometer (TU-1901, Pgeneral, China). Electrochemical impedance

119

spectroscopy (EIS) was performed to determine the conductivity of the electrodes, with the

120

frequency ranging from 10-3 to 105 Hz, and the potential was 1V. The electrolyte was 0.005 M

121

[Fe(CN)6 3-]/[Fe(CN)6 4-] solution.

Ac ce p

114

122

Photoelectrochemical properties are measured in a rectangular shaped quartz reactor

123

(20mm×30mm×50mm). The setup mainly consists of external irradiation source, three-electrode 6 Page 6 of 28

configuration and data recording system. A computer controlled electrochemical station (CH Ins.,

125

CHI660, USA) was used to apply the bias potential and record the photocurrent. The as-prepared

126

samples worked as the work electrode, a platinum foil was counter electrode and a saturated

127

Ag/AgCl was reference electrode in a solution containing 0.2 M Na2SO4. An external Xenon lamp

128

with AM 1.5 (a radiation intensity of 100 mW cm-2) is used as light source. The visible light was

129

obtained by a glass filter that allowed wavelengths between 380 and 800 nm to be passed through.

130

2.4 PEC degradation experiment

us

cr

ip t

124

The PEC degradation experiment of TC setup under visible light and solar light is the same as

132

PEC setup. The degradation experiment conditions were as follows: illumination area 10mm×10 mm,

133

and 0.5V (vs. Ag/AgCl) of electric bias, pH 5.5, 0.2 M Na2SO4 as electrolyte. The initial

134

concentration of TC solution was 20 mg L−1 and the reaction solution was 20 mL. During the

135

degradation experiments, the stirring was done by the magnetic stirring with a small magnetic stirrer.

136

The reaction solution (~3mL) was quickly withdrawn at given reaction intervals, and was quickly

137

returned to the reactor after being analyzed with a spectrophotometer (UV759, Shanghai) at 352 nm.

138

3. Results and discussions

139

3.1 Surface microtopography and structure of the electrodes

Ac ce p

te

d

M

an

131

140

Figure 1 a–d depicts the formation of the ternary n-ZnO/p-Cu2O /n-TNA electrodes featured in this

141

work. First, highly ordered TiO2 nanotube arrays were synthesized via an anodization process

142

following calcination at 450°C to transfer amorphous TiO2 into anatase (Fig.1b). Second, Cu2O was

143

deposited on the TNAs by electrochemical deposition (Fig.1c). Third, ZnO nanowires were

144

overlayed on the top of the p-Cu2O/n-TNA by a hydrothermal method (Fig.1d).

145

In order to confirm the composite electrode, FE-SEM was conducted to investigate the 7 Page 7 of 28

morphology change of electrode. It can be seen from Fig. 2a that highly ordered TNAs were

147

fabricated after a typical anodization in HF-H2O electrolyte. The typical pore size is ranging from

148

80-100 nm with an average interstice of 10 nm. The electrochemical deposited Cu2O were shown in

149

Fig. 2b. The Cu2O nanoparticles had uniform size and were mostly octahedral structure. Although

150

most of Cu2O nanoparticles were found on the top of the nanotubes due to their narrow pore size,

151

considerable amount of them also were embedded in the tube mouth. This could offer the comparable

152

contact region between Cu2O nanoparticles and TNAs so as to improve the electro-hole pair

153

separation. Fig. 2c presents the morphology of ZnO nanowires after hydrothermal growth. It is

154

apparent that ZnO nanowires have a high degree of orientation with the c-axis vertical to the

155

substrate surface. The cross-section further demonstrates the ternary structure of the composite

156

electrode as shown in Fig. 2d. As expected, ZnO nanowires grown on the top of the TNAs

157

representing an obvious two-tier architecture, whereas the Cu2O nanoparticles should be wrapped by

158

the TNAs and ZnO NWs. It also demonstrated that the ZnO nanowires have fully covered the surface

159

of electrode that can protect the Cu2O particles from phototcorrosion.

Ac ce p

te

d

M

an

us

cr

ip t

146

160

Fig. 3 corresponds to the X-ray diffraction (XRD) patterns of pure TNA, p-Cu2O/n-TNA,

161

n-ZnO/p-Cu2O/n-TNA respectively. It can be seen from pattern (curve a) that the sample possesses

162

characteristic peaks at 25.3°(101), 38.1° (004), and 48.2° (200) for the anatase phase. After coupling

163

with Cu2O, the sample clearly shows additional characteristic peaks of Cu2O at 29°, 37° (curve b).

164

The ternary heterojunction n-ZnO/p-Cu2O/n-TNA was approved by the new dominant diffraction

165

peak (curve c), which indicates corresponding to the ZnO nanowires to be a high degree of

166

orientation with the c-axis vertical to the substrate surface.

167

Fig. 4a gives the X-ray photoelectron spectroscopy (XPS) survey scan over a large energy range 8 Page 8 of 28

at low resolution of n-ZnO/p- Cu2O/n-TNA material, which represents Ti, Cu, Zn and O. Fig. 4b

169

shows the Zn 2p core level XPS scans, at higher resolution over smaller energy windows. As can be

170

seen, the Zn 2p core level XPS spectrum has two sharp peaks at1022.5 eV (Zn 2p3/2) and 1045.6

171

eV(Zn 2p1/2), which is in good agreement with the reported values for ZnO.

172

3.2 The PEC activity of electrodes

cr

ip t

168

The UV/Vis diffuse reflection spectra (DRS) of TNA, p-Cu2O/n-TNA, n-ZnO/p-Cu2O/n-TNA

174

are given in Fig. 5. It is evident that the pure TNA electrode has no obvious absorption of visible

175

light (curve a). The absorption band is 375 nm and band gap is about 3.20 eV (curve a), according to

176

the equation: Eg= 1240/λg. As shown in curve b, the absorption edge of p-Cu2O/n-TNA is observed

177

at the wavelength 505 nm, corresponding to a band gap of 2.48eV, indicating that the deposition of

178

Cu2O for TNA extend the absorption range to the visible region. As can be seen from curve c, the

179

band gap absorption edge of the ternary n-ZnO/p-Cu2O/n-TNA is similar to that of p-Cu2O/n-TN

180

and extends the visible spectrum absorption (to 510 nm), corresponding to an Eg value of about 2.43

181

eV. Under illumination of visible light, the slight red-shifted of the band gap absorption and the

182

change in Eg may be ascribed to the growth ZnO on p-Cu2O/n-TNA, which can protect the Cu2O

183

from photocorrosion and facilitate kinetic separation of photogenerated charges. The results suggest

184

that the coupling of n-ZnO with binary heterojunction p-Cu2O/n-TNA could be more efficient in

185

solar light harvest.

Ac ce p

te

d

M

an

us

173

186

Further investigation was carried out to compare the current density generated by the TNA

187

electrode, p-Cu2O/n-TNA electrode, and n-ZnO/p-Cu2O/n-TNA electrode under visible light (Fig. 6).

188

The dark current densities of these three electrodes are found to be negligible. However, the pure

189

TNA also shows no obvious light response in the visible light region, indicating no electron/hole pair 9 Page 9 of 28

was induced by visible light. After the chemically assembled sensitization by Cu2O, The

191

p-Cu2O/n-TNA electrode increases the photoelectrocatalytic activity under visible light. In addition,

192

the n-ZnO/p-Cu2O/n-TNA electrode exhibits the higher visible light response. At an applied potential

193

of 0.5 V, the current density is 0.83mA cm-2, which is 106 times as high as the pure TNA electrode

194

and 3.6 times the p-Cu2O/n-TNA electrode.

cr

ip t

190

Fig. 7 shows a schematic illustration of the band-gap energy and the charge separation of the

196

ternary n-ZnO/p-Cu2O/n-TNA electrode. The CB of Cu2O is more negative than that of TiO2 and

197

ZnO. Therefore, the photoelectron transfer may occur from the CB of Cu2O towards the CB of ZnO,

198

then to that of TiO2, while the photogenerated holes transfer may occur in the opposite direction.

199

Between the bands of TiO2 and Cu2O, ZnO acts as the beneficial role of the intermediate stage that

200

would greatly promote the hole electron transfer, thus reducing the chance of hole–electron

201

recombination. Therefore, the ternary n-ZnO/p-Cu2O/n-TNA has the higher photocatalytic

202

properties than the pure TNA and binary p-Cu2O/n-TNA.

te

d

M

an

us

195

EIS is a high effective method for probing the photoelectrochemical characterization of

204

surface-modified electrodes. In this study, EIS was carried out to investigate the changes of electron

205

transfer resistance that aroused from every surface modification step as shown in Fig. 8. The pure

206

TNA electrode exhibits poor conductivity with an EIS of about 1000 Ω. After deposited with Cu2O

207

(curve b), the EIS of p-Cu2O/n-TNA electrode shows a small semicircle (250Ω), only about a quarter

208

of that of pure TNA, which suggests the successful deposition of Cu2O on the TNA electrode. The

209

EIS of the ternary n-ZnO/p-Cu2O/n-TNA is similar to that of p-Cu2O/n-TNA (curve c), which may

210

be attributed to the better transfer and dispersion due to the TNA surface coating with Cu2O and

211

ZnO.

Ac ce p

203

10 Page 10 of 28

212 213

3.4 PEC degradation of TC under visible light and solar light PEC

degradations

of

TC

using

TNA

electrode,

p-Cu2O/n-TNA

electrode

and

n-ZnO/p-Cu2O/n-TNA electrode under visible light and solar light were present in Fig. 9a and Fig.

215

9b, respectively.

ip t

214

As given in Fig. 9a, within 3 h, the removal percentage of TC on pure TNA electrode is

217

obviously much slower than that of p-Cu2O/n-TNA electrode and n-ZnO/p-Cu2O/n-TNA electrode.

218

The pure TNA exhibit no obvious light response in the visible-light region. A rapid increase in the

219

removal percentage of TC can be obtained on p-Cu2O/n-TNA electrode, where the removal

220

percentage reaches 75 %. However, the n-ZnO/p-Cu2O/n-TNA also shows the highest

221

photoelectrocatalytic activity, with a removal percentage of 85 % after 3 h degradation. Further

222

investigations were carried out under solar light and the results were present in Fig. 9b. Comparing

223

the degradations data under visible light, an obvious increase in the removal percentage of TC by

224

pure TNA electrode can be observed. The n-ZnO/p-Cu2O/n-TNA also shows the highest

225

photoelectrocatalytic activity, with a removal percentage of 90% after 3 h degradation, indicating an

226

excellent photoelectrocatalytic activity in both the visible light and solar light of ternary

227

n-ZnO/p-Cu2O/n-TNA. In addition, the terminal pH of reaction solution degraded by ternary

228

n-ZnO/p-Cu2O/n-TNA electrode was also determined. The terminal pH value of reaction solution

229

under visible light is 5.89 and under solar light is 5.84, respectively, which are close to the initial pH

230

value of 5.5. The small change of pH value may be ascribed to the presence of some small molecular

231

compounds during the degradation, which act as the buffer solution to keep the relative stable pH

232

value of reaction solution.

Ac ce p

te

d

M

an

us

cr

216

11 Page 11 of 28

After first being deposited by the Cu2O and then coated by ZnO, the ternary heterojuncrion

234

n-ZnO/p-Cu2O/n-TNA electrode has a broad-wave response in the visible light region, indicating that

235

the separation of photogenerated holes and electron was promoted. This charge separation prevented

236

the photoinduced electron and the hole from recombination and consequently leads to higher

237

degradation efficiency. The results indicate that the n-ZnO/p-Cu2O/n-TNA photocatalyst is optimal

238

for the oxidation of organic pollutants.

239

3.4 The stability of three electrodes 10

shows

the

stability

cr of

TNA

us

Fig.

electrode,

p-Cu2O/n-TNA

electrode

and

an

240

ip t

233

n-ZnO/p-Cu2O/n-TNA electrode for treatment of TC under solar light. As can be seen from Fig. 9,

242

the results of the 4 repeated experiments for degradation of TC in 3 h shows that the degradation

243

efficiencies using TNA electrode is stable with an average degradation efficiency of 72.5 ± 1.2 %.

244

This indicates that TNAs electrode processes excellent stability and reliability. However, the

245

removal percentage is 85 % at the beginning and decreases quickly to 75 % after 4 repeated

246

experiments for degradation of TC using p-Cu2O/n-TNA electrode, which is due to the

247

photocorrosion

248

n-ZnO/p-Cu2O/n-TNA electrode decreased slightly with the repeated times, removal percentage of

249

TC still reaches 85 % after 4 repeated experiments, indicating higher stability after depositing the

250

ZnO on the surface of p-Cu2O/n-TNA. The higher removal percentage and stability might be

251

explained by the following two reasons. One is that the coupled n-ZnO/p-Cu2O/n-TNA photoanode

252

might facilitate kinetic separation of photogenerated charges and decreases the recombination rate

253

within the electrode. Another is that the ZnO coating on p-Cu2O/n-TNA electrode can protect Cu2O

254

from photocorrosion.

Ac ce p

te

d

M

241

of

Cu2O

particles.

Although

the

removal

percentage

of

TC

using

12 Page 12 of 28

255

4. Conclusions In summary, a novel n-ZnO/p-Cu2O /n-TNA material with higher photocatalytic efficiency and

257

stability was designed and applied to degrade TC. The coupled n-ZnO/p-Cu2O/n-TNA photoanode

258

might facilitate kinetic separation of photogenerated charges and decreases the recombination rate

259

within the electrode. Moreover, the ZnO coating on p-Cu2O/n-TNA electrode can protect Cu2O from

260

photocorrosion. The ternary heterojunction n-ZnO/p-Cu2O/n-TNA electrode offers higher

261

photocatalytic efficiency during the PEC process, and thus obtains much higher degradation

262

efficiency in comparison to the pure TNA and binary p-Cu2O/n-TNA electrode. The results also

263

show that the ternary heterojunction n-ZnO/p-Cu2O/n-TNA electrode possesses excellent stability

264

and reliability during the serial experiments. Since the Cu2O was protected against photocorrosion in

265

solution by coating a layer of n-ZnO ontop the p-Cu2O/n-TNA surface. The enhanced

266

photoelectrochemical properties and mechanical stability of the composite electrode material make it

267

a highly efficient photoanode material for various potential applications.

268

Acknowledgement

269

The authors would like to acknowledge the National Nature Science Foundation of China (No.

270

21207088,

271

(No.20110073110029), and the Shanghai Basic Research Key Project (11JC1406200), the State Key

272

Development Program for Basic Research of China (Grant No. 2009CB220004) for financial support,

273

and Instrumental analysis center of Shanghai Jiao Tong University for materials characterization.

274

Reference

275

[1] Y. H. Xu, D. H. Liang, M. L. Liu, D. Z. Liu, Preparation and characterization of Cu2O–TiO2:

276

Efficient photocatalytic degradation of methylene blue, Mater. Res. Bull. 43(2008)3474–3482.

Ac ce p

te

d

M

an

us

cr

ip t

256

21177085),

Doctoral

Program

of

the

Ministry

of

Education

of

China

13 Page 13 of 28

[2] E. Evgenidou, K. Fytianos, I. Poulios, Semiconductor-sensitized photodegradation of dichlorvos

278

in water using TiO2 and ZnO as catalysts, Appl. Catal. B.59(2005)81–89.

279

[3] Q. L. Huang, G. Zhou, L. Fang, L. P. Hu, Z. S. Wang, TiO2 nanorod arrays grown from a mixed

280

acid medium for efficient dye-sensitized solar cells, Energy Environ. Sci. 4(2011)2145–2151.

281

[4] A. Fujishima, X.T. Zhang, Titanium dioxide photocatalysis: present situation and future

282

approaches, C. R. Chimie. 9(2006)750–760.

283

[5] M. F. Bregmera, K. Rajeshwar and M. V. B. Zanoni, Bisphenol A removal from wastewater using

284

self-organized TiO2 nanotube array electrode, chemosphere. 78(2010) 569-575.

285

[6] J. Georgieva, E. Valova, S. Armyanov, N. Philippidis, I. Poulios, S. Sotiropouloss, Bi-component

286

semiconductor oxide photoanodes for the photoelectrocatalytic oxidation of organic solutes and

287

vapours: A short review with emphasis to TiO2–WO3 photoanodes, J. Hazard. Mater. 211-212(2012)

288

36-46.

289

[7] Y. X. Li, C. F. Xie, J. Mol, Eosin Y-sensitized nitrogen-doped TiO2 for efficient visible light

290

photocatalytic hydrogen evolution ,

291

Enhancement of photocatalytic activity of sprayed nitrogen-containing ZnO powders by coupling

292

with metal oxides during the acetaldehyde decomposition, Chemosphere. 54(2004)1099–1110.

293

[8] J. K. Yang, X. T. Zhang, H. Liu, C. H. Wang, S. P. Liu, P. P. Sun, L.L. Wang, Y. C. Liu,

294

Heterostructured TiO2/WO3 porous microspheres: Preparation, characterization and photocatalytic

295

properties, Catal. Today. 201(2013) 195–202.

296

[9] C. Wang, X.M. Wang, B.Q. Xu, J.C. Zhao, B.X. Mai, P.A. Peng, G. Y. Sheng, J. M. Fu,

297

Enhanced photocatalytic performance of nanosized coupled ZnO/SnO2 photocatalysts for methyl

298

orange degradation, J. Photochem. Photobiol. A. 168(2004)47–52.

Ac ce p

te

d

M

an

us

cr

ip t

277

Catal. A: Chem. 282(2008)117–123. [6]D. Li, H. J. Haneda,

14 Page 14 of 28

[10] S. Sakthivel, S.U. Geissen, D.W. Bahnemann, V. Murugesan, A. Vogelpohl, Enhancement of

300

photocatalytic activity by semiconductor heterojunctions: α-Fe2O3, WO3 and CdS deposited on ZnO,

301

J. Photochem. Photobiol. A. 148 (2002)283–293.

302

[11] D. Li, H. Haneda, Photocatalysis of sprayed nitrogen-containing Fe2O3–ZnO and WO3–ZnO

303

composite powders in gas-phase acetaldehyde decomposition, J. Photochem. Photobiol. A.

304

160(2003)203–212.

305

[12]A. Fujishima, X. T. Zhang, D. A. Tryk, Heterogeneous photocatalysis: From water photolysis to

306

applications in environmental cleanup, Int. J. Hydrogen. Energy. 32(2007)2664-2672.

307

[13] J. J. Kleber, G. R. Helz, Indirect photoreduction of aqueous chromium(VI), Environ. Sci.

308

Technol. 26(1992)307–312.

309

[14] I. Eswaramoorthi, V. Sundaramurthy, A.K. Dalai, Partial oxidation of methanol for hydrogen

310

production over carbon nanotubes supported Cu-Zn catalysts, Appl. Catal. A. 313 (2006)22–34.

311

[15] H. C. Yang, F. W. Chang, L.S. Roselin, Hydrogen production by partial oxidation of methanol

312

over Au/CuO/ZnO catalysts, J. Mol. Catal. A: Chem. 276(2007)184–190.

313

[16] Z. L. Liu, J. C. Deng, Fabrication and photocatalysis of CuO/ZnO nano-composites via a new

314

method, Mater. Sci. Eng. B 150(2008)99–104.

315

[17] H. Zhu, B. Yang, J. Xu, Z. Fu, M. Wen, T. Guo, S. Fu, J. Zuo, S. Zhang, Construction of

316

Z-scheme type CdS–Au–TiO2 hollow nanorod arrays with enhanced photocatalytic activity, Appl.

317

Catal. B. Environ. 90(2009) 463–469.

318

[18] S. Yamada, A.Y. Nosaka, Y. Nosaka, Fabrication of CdS photoelectrodes coated with titania

319

nanosheets for water splitting with visible light, J. Electr. Chem. 585(2005)105–112.

Ac ce p

te

d

M

an

us

cr

ip t

299

15 Page 15 of 28

[19] P. E. de Jongh, D. Vanmaekelbergh and J. J. Kelly, Photoelectrochemistry of Electrodeposited

321

Cu2O, J. Electrochemi. Soc. 147(2000)486–489.

322

[20] Helaı¨li A, Y. Bessekhouad, A. Bouguelia a, M. Trari, p-Cu2O/n-ZnO heterojunction applied to

323

visible light Orange II degradation, Solar. Energy. 84 (2010)1187–1192.

324

[21] C. Xu, L. X. Cao, G. Su, W. Liu, H. Liu, Y. Q. Yu, X. F Qu, Preparation of ZnO/Cu2O

325

compound photocatalyst and application in treating organic dyes, J. Hazard. Mater. 176

326

(2010)807–813.

327

[22] A. Paracchino, V. Laporte, K. Sivula, M. Grätzel and E.Thimsen, Highly active oxide

328

photocathode for photoelectrochemical water reduction, Nature Mater. 10(2011)456–461.

329

[23] Y. B. Liu, H. B. Zhou, B. X. Zhou, J. H. Li, H. C. Chen, D. Li, W. M. Cai, Enhanced

330

Photoelectrochemical Properties of Cu2O-loaded Short TiO2 Nanotube Array Electrode Prepared by

331

Sonoelectrochemical Deposition, Nano.Micro. Lett. 2(2010) 277–284.

332

[24] J. L. Zhang, B. X. Zhou, Q. Zheng, J. H. Li, J. Bai, Y. B. Liu, W. M. Cai, Photoelectrocatalytic

333

COD

334

43(2009)1986–1992.

335

[25] J. Bai, J. H. Li, Y. B. Liu, B. X. Zhou, W. M. Cai, new glass substrate photoelectrocatalytic

336

electrode for efficient visible-light hydrogen production: CdS sensitized TiO2 nanotube arrays, Appl.

337

Catal. B. Environ. 95(2010)408–413.

method

using

Ac ce p

determination

te

d

M

an

us

cr

ip t

320

highly

ordered

TiO2 nanotube

array,

Water

Res.

16 Page 16 of 28

Figure captions Figure 1 Schematic illustration of the structure of the ternary n-ZnO/p-Cu2O/n-TNA Figure 2 FE-SEM images of the electrodes: (a) TNA electrode after anodization for 30min; (b) after

ip t

Cu2O sonoelectrochemical deposition for 5 min; (c) and after ZnO hydrothermal deposition for 4 h

cr

Figure 3 XRD patterns of: (a) TNA; (b) p-Cu2O/n-TNA; (c)n-ZnO/p-Cu2O/n-TNA

of n-ZnO/p-Cu2O/n-TNA electrode UV/Vis

diffuse

reflection

spectra

(DRS)

of

TNA,

p-Cu2O/n-TNA

and

an

Figure5

us

Figure 4 (a) XPS survey scan for n-ZnO/p-Cu2O/n-TNA electrode; (b) Zn 2p XPS core level spectra

n-ZnO/p-Cu2O/n-TNA

M

Figure 6 Photocurrent density of TNA electrode, p-Cu2O/n-TNA electrode, n-ZnO/p-Cu2O/n-TNA electrode

n-ZnO/p-Cu2O/n-TNA

te

d

Figure 7 Schematic illustration of the band gap energy and charge separation of the ternary

Ac ce p

Figure 8 Electrochemical impedance spectroscopy of three electrodes: (a) TNA; (b) p-Cu2O/n-TNA; (c)n-ZnO/p-Cu2O/n-TNA

Figure 9 (a) PEC degradation of solutions of TC by TNA electrode, p-Cu2O/n-TNA electrode, n-ZnO/p-Cu2O/n-TNA electrode under visible light; (b) PEC degradation of solutions of TC by TNA electrode, p-Cu2O/n-TNA electrode, n-ZnO/p-Cu2O/n-TNA electrode under solar light Figure 10 Durability of by TNA electrode, p-Cu2O/n-TNA electrode, n-ZnO/p-Cu2O/n-TNA electrode for degradation of TC

17 Page 17 of 28

Highlights The TNA as the substrate exhibits better charge separation and transfer in UV region. The coupling of TNA with Cu2O extends the visible spectrum absorption.

Ac ce p

te

d

M

an

us

cr

ip t

The coupling of ZnO with Cu2O/TNA protects the Cu2O from photocorrosion .

18 Page 18 of 28

Ac

ce

pt

ed

M

an

us

cr

i

Figure 1

Page 19 of 28

Ac

ce

pt

ed

M

an

us

cr

i

Figure2

Page 20 of 28

Ac

ce

pt

ed

M

an

us

cr

i

Figure3

Page 21 of 28

Ac

ce

pt

ed

M

an

us

cr

i

Figure4

Page 22 of 28

Ac

ce

pt

ed

M

an

us

cr

i

Figure 5

Page 23 of 28

Ac

ce

pt

ed

M

an

us

cr

i

Figure 6

Page 24 of 28

Ac

ce

pt

ed

M

an

us

cr

i

Figure 7

Page 25 of 28

Ac

ce

pt

ed

M

an

us

cr

i

Figure 8

Page 26 of 28

Ac

ce

pt

ed

M

an

us

cr

i

Figure 9

Page 27 of 28

Ac

ce

pt

ed

M

an

us

cr

i

Figure 10

Page 28 of 28