Review of magnetic methods for nondestructive evaluation (Part 2)

Review of magnetic methods for nondestructive evaluation (Part 2)

Review of magnetic methods for nondestructive evaluation ( Part 2) D.C. Jiles This paper gives a guideline to the literature of magnetic methods for n...

1MB Sizes 3 Downloads 140 Views

Review of magnetic methods for nondestructive evaluation ( Part 2) D.C. Jiles This paper gives a guideline to the literature of magnetic methods for nondestructive evaluation of materials for flaws and defects. This is a sequel to an earlier paper which described magnetic methods for nondestructive evaluation of stress, plastic deformation and microstructure. The present paper discusses magnetic particle inspection, magnetic flux leakage, leakage field calculations and eddy current inspection, including the remote field electromagnetic inspection method. An extensive survey of recent publications in the field is given.

Keywords:magnetic methods, flaws, defects, magnetic particle inspection, magnetic flux leakage, leakage field calculations, eddy current inspection, remote field electromagnetic inspection

The subject of this review is nondestructive evaluation of defects or flaws in ferromagnetic steels. This paper is a sequel to the review of magnetic methods for nondestructive evaluation of intrinsic, ie non-flaw-related, properties of ferromagnetic materials tl]. As in the earlier paper, the objective of the review is to provide a broad survey of the existing literature, giving a comprehensive summary of earlier work but without going into fine details, which have been covered in most cases by more specialized reviews of the particular techniques. The subject of flaw detection in materials using magnetic methods has a long history, going back as far as Saxbyt2] in the last century. Systematic development of testing techniques based on perturbations of the magnetic flux in iron and steel due to the presence of defects did not begin, however, until after the chance discovery of Hoke t3] that iron filings accumulated close to defects in hard steels while in the process of being ground. The technique of magnetic particle inspection, which was based on this discovery, was then developed by deForest t4] and Donne ts]. Later, as the subject of flaw detection became more quantitative, additional methods were developed in which the leakage field in .the vicinity of the flaw was measured with a magnetometer. Once the field strengths of the leakage fields were being measured on a routine basis, it became desirable to relate these to flaw size and shape, and therefore there arose the need for modelling the leakage fields from different crack geometries.

to deForest to develop the method further for practical use. DeForest's work involved devising methods of generating a magnetic field of sufficient strength in any direction in a specimen. This he solved by proposing that electrical contact electrodes (known as 'prods') with heavy-duty cables be used to pass large currents through test specimens in desired directions. Furthermore, he realized the need to use magnetic powders with uniform properties such as particle shape, size and saturation magnetization in order to obtain more reliable and reproducible results. DeForest and Donne formed the Magnaflux Corporation lrJ to exploit the MPI method in 1934. This company remains one of the principal suppliers of equipment for MPI. The MPI method is very simple in principle. It depends on the leakage of magnetic flux at the surface of a ferromagnetic material in the vicinity of surface-breaking or near-surface flaws (Figure 1). There are two main methods for generating a magnetic field in a material: the 'yoke' method and the 'prod' method. A magnetic yoke wound with a field coil can be used, as shown in Flux lines are perturbed near flaw

~

Magnetic particle accumulation

Magnetic particle inspection (MPI) The technique of magnetic particle inspection was the first magnetic NDE method in widespread use. It was discovered accidentally by Hoke in 1918, but it was left

flux Fig. 1 Schematic diagram of leakage flux in the vicinity of a surface-breaking flaw with accumulation of magnetic particles

0308-9126/90/020083-10 © 1990 Butterworth & Co (Publishers) Ltd NDT International Volume 23 Number 2 April 1990

83

Power cables

Electro

Specimen Fig. 2

Flow

The magnetic yoke method for magnetizing a material

Figure 2. Alternatively, a high electric current can be passed through the component using contact electrodes ('prods'). The current generates a circulating magnetic field as given by the right-hand rule (corkscrew rule). In both cases the best indication is given when the magnetic field is perpendicular to the largest dimension of the flaw or crack. It is a very reliable method, when used correctly, for finding these surface or near-surface flaws and gives a direct indication of the location and length of the flaw. There is little or no limitation on the size or shape of component being tested, although more care is needed in the application of the method to complex geometries. Nevertheless, the method does have some distinct limitations. It can of course only be used on ferromagnetic materials, and in addition the magnetic field must lie perpendicular to the direction of the flaw to give the best indication. Flaws can easily be overlooked by misorientation of the field. Finally, although the length of the flaw is easily found, the depth is difficult to ascertain. Although some indications of flaw depth based on the amount of powder accumulated at the crack or flaw have been suggested, these are not entirely satisfactory, Various enhancements have been made to the original 'dry powder method'. These include the use of waterborne suspensions or magnetic inks, known as the 'wet method', and also fluorescent powders which often give a clearer indication of small flaws when viewed under ultraviolet light. Another method that has found use in detection of flaws in structural components is the 'replica' or magnetographic method in which a magnetic tape is placed over the area to be inspected t71. The tape is magnetized by the strong surface field and is then removed and inspected for magnetic anomalies. The magnetic tape, which records an imprint of the flux leakage from the surfaces of components, can be inspected afterwards using magnetometers such as Hall probes or fluxgates. The advantage of this method over the magnetic particle inspection technique is that the magnetograph (usually a magnetic tape) can be read using a magnetometer to obtain a quantitative measure of flux leakage from regions where it would be difficult to use a magnetometer, e9 inside pipelines or for underwater applications.

certainly not reproducible and are likely to be unreliable for other reasons such as the lack of control over the relative orientation of field and flaw. Therefore it is standard procedure to apply a controlled magnetic field to the specimen, either through a magnetic yoke or by the prod magnetization method. Recently much of the research effort in MPI has been directed towards establishing standard procedures and conditions for applying the method. Gregory et al tSJ have shown that for complex geometries the magnetic particle method is less successful and has sometimes failed to reveal structural faults in aerospace components because of less magnetization in some regions of those components. Optimum conditions for the application of MPI to inspection of welds were described by Massa 191. Once again the critical factor was to determine adequate levels of magnetization in order to reveal the presence of defects. No simple solution was found in that case, but tables of values of critical field strength H for various geometries were given. Some standard procedures have been recommended in the UK t1°1, where a field strength of at least 30 Oe (2400 A m -x) was suggested for using MPI on steels. However, opinions seem to differ over the necessity of the recommendation. Work on MPI applications to pressure vessels and pipelines by Raine et al tl q has shown that the recommendations of BS 6072 do not seem to be generally applicable. Their work indicated that field strengths lower than 30 Oe were quite adequate for satisfactory MPI indications. Edwards and Palmer have investigated procedures for applying the method to tubular slSecimens threaded on a current-carrying conductort12~ (Figure 3) and for a cylindrical bar using prod magnetizationtl 3]. It was shown that care is needed to generate sufficient field strength for adequate magnetization of the specimen in these cases. Often it is most convenient to use an electromagnet to get an adequate magnetic field in the testpiece, as shown in Figure 2. It is sometimes assumed that the optimum magnetizing condition corresponds to the maximum permeability; however, this was not found to be true in the work of Oehl and Swartzendrubert141. They found that for cylindrical defects with square cross-sections the ratio of leakage field to applied field reached a maximum at an applied field of between 10 and 30 Oe in steels, depending on the lift-off. This was well removed from the maximum

Applications of the M P I method Although it is possible to apply the MPI technique solely on the remanent magnetization of a specimen and its accompanying field, the results obtained in this way are

84

Fig. 3 Magnetizing a hollow tube specimen using the threaded tube method. A conductor carrying a current / (A) is threaded through the specimen

NDT International April 1990

permeability H = 1.50e.

of the

material,

which

occurred

at

Forster tT] has described the use of the magnetographic method for the detection of flaws on the inside surfaces of tubes and in pipe welds. A recent enhancement of the fluorescent MPI method has been reported by Chen t15], who used automated scanning of steel components for crack indications followed by digital image-processing techniques to enhance the results. The automation of the inspection method has the advantage of eliminating subjective evaluation of results and is therefore desirable. The 'wet method' in which a magnetic colloid is used has many similarities with the Bitter pattern technique for magnetic domain observations. Because of the finer particles used in the wet method, it has some advantages in spatial resolution over the dry powder method and therefore can be successfully used for detection of smaller flaws. The next stage of the evolution of MPI should be the development of expert systems, since even with automated measurement there are some disadvantages compared with a human operator. For example, an experienced inspector will know where flaws are most likely to occur and therefore can concentrate his efforts on that area. The transfer of this expertise to computer systems would be advantageous. In conclusion, therefore, MPI is a well established technique and most of the problems associated with it appear to have been solved. The remaining research effort is directed towards optimizing conditions for its use. A review of magnetic particle inspection was given by Bezer/16'17] some years ago. More recent reviews of the subject have been given by Bezert~s] and Dunn tt9], who have provided introductory surveys of the field. The standard reference work on MPI is Principles of Magnetic Particle Testing by Betz/2°], which contains much information on the subject, including the history of its development, the underlying principles, methods of generating fields in the materials and descriptions of the dry powder methods, the wet (or magnetic ink) method and the fluorescent powder method.

Magnetic flux leakage (MFL) The magnetic flux leakage method is derived from the magnetic particle inspection method. Both depend on the perturbation of magnetic flux in a ferromagnetic material caused by surface or near-surface flaws. Whereas in the MPI method detection relies on the accumulation of magnetic powder, or sometimes the use of a magnetic recording tape [21'22], to indicate the presence of a defect, the flux leakage technique utilizes a magnetometer. The use of a magnetometer for detecting leakage fields was first suggested by Zuschlag t23]. The magnetometer allows a quantitative measurement of the leakage field in the vicinity of a flaw to be obtained. Furthermore, the field components in three directions, perpendicular and parallel to the flaw and normal to the surface, can be measured, although in practice only components parallel to the surface are usually measured. However, the method only began to gain wide acceptance after the design of a practical flux-leakage-measuring system by Hastings t24,2s].

NDT International April 1990

This was capable of detecting surface and subsurface flaws on the inner surface of steel tubes, a location that was quite unsuitable for the MPI method. The flux leakage technique has now been further developed so that it can be used not only for the detection of flaws but also for their characterization t26'271. The magnetometer probe is most often a Hall probe or induction coil. It is scanned across the surface of the component looking for anomalies in the flux density which indicate the location of a flaw, as in Figure 4. The leakage flux as a function of distance across a crack is shown in Figure 5, together with a typical search coil output as it is moved across the crack. A drawback of this method compared with the particle method is that while large areas of material can be tested quickly using MPI, the scanning of a magnetometer over the surface can be time-consuming. Therefore the flux leakage method has advantages in situations where the location of flaws is known or where the location can be predicted with a reasonable chance of success. Under those circumstances a careful magnetic inspection can be conducted over a confined area. Another situation when flux leakage magnetometry has advantages over the particle method is where the part to be tested is not easily accessible for a visual inspection. An example is the inside surfaces of long tubes and pipelines t2a]. Once again, under these circumstances, magnetic flux leakage magnetometry has been an important and highly successful technique for detection of both flaws and stresses t29]. Subsequent work on detection of flux anomalies in pipelines indicated that these could be related to stresses within the pipe wall t3°'aH. The method has been particularly useful for the inspection of defects in underground pipelines, as in the work of Atherton t321 and Khalileev and co-workers [33'34]. Magnetometer scanning surface J J of component ~/

\

//

/

~

Ia

~

%

~

Flux lines are

perturbednear flaw

a

\

,

near recjionof lower Jpermeability causing

Jflux

Hall

probe

anomaly

:

/

Mogn~ic flux /

-"

(

/ Lower- permeability

material

Hiqh - permeability material

b Fig. 4 Scanning the surface of a specimen with a magnetometer (a) to detect flaws and (b) to detect regions of low permeability by the magnetic flux leakage method

85

30 Flux

3000 ~7777777"277"777777

~

2ooo

0.5

2o 2000

-J

0

0 0

l

I

2

4

I

6

Position of coil (ram)

I

8

IO

o

0.8 , I

-- I0

I000--

LE

2.5

3 0

~ -10

1.2

IO00

0

~

,~

//

2

I

I

~.-- Inside Crack

. ~

2 3 Height h (rnm)

Outside Crack

P

a

Search coil output -20

/ = 8o1-1

/

_ _ 91

30 Fig. 5 Variation of leakage flux with distance across a crack (after Beissner et a/[43] )

As with the MPI method, the flux leakage signal depends on the level of magnetization within the material. Pashagin et al t351 have also shown that it depends on the method of magnetization, such as magnetizing by current flow or via magnetizing coils. Introductory reviews of the flux leakage method t36,37J and also a more advanced review t3m have been given by Forster. These discuss both the experimental and theoretical foundations of the method. The demagnetizing fields Hd of defects were calculated for ellipsoidal flaws inside the material, and consequently the true internal field in the defect, Hi, was calculated from the measured applied field H~ using the equation H i = H~ - Hd

Once again this procedure is equivalent to assuming that the defect behaves like a simple magnetic dipole. Such an assumption is only valid as a first approximation. If the permeability of the material is #=~o., the permeability of the flaw is #haw and the demagnetizing factor, which depends on the shape of the flaw, is N d, then the internal field is Hi =

fliron

Ha

/'/iron + Nd(//flaw + fliron)

One of the difficulties here is that of course in general the magnetic induction in a ferromagnet is not known as a function of field H and hence #=ro, is not known as a function of H. These reviews were completed with experimental results on the variation of leakage flux with lift-off position above the crack and also as a function of depth within the crack, as shown in Figure 6. These showed that as the lift-offdistance increased, the leakage field became insensitive to crack depth at lift-offdistances above 1 mm for crack depths of 2.5 mm with varying widths of 0.2-2 mm.

86

Height h (mm) ~_

InsideCrack

,_.

Outside Crack

.

b Fig. 6 Variation of leakage field with position within and above a crack for various crack widths (after Forster[~'37] ) :(a ) carbon steel; (b) chromium steel

Applications of the flux leakage method Stumm [391has described several devices based on the flux leakage technique which can be used for testing of ferromagnetic tubes for flaws. One of the problems identified with these instruments was the difference in defect signal between an external (near-side) flaw and an internal (far-side) flaw. The signal from an internal flaw was much smaller than the signal from a comparable external flaw or a much larger internal flaw. One device, called the 'rotomar, enabled the tube to be passed through a rotating magnetizing yoke which generated a circumferential magnetic field for detecting longitudinal defects in the tube wall. The leakage flux was measured using an array of Hall probes. Tube diameters of 20-450 mm could be inspected. A second instrument, the 'tubomar, rotated the tube while maintaining the detection system stationary. The detection and field generation systems were identical to those used in the rotomat system. The method of magnetization, however, was dependent upon the size of the pipe. For large pipes the pipe was threaded with a central conductor which then carried the current required to obtain the optimum field strength in the pipe wall. For smaller pipes the magnetic yoke method was employed.

NDT International April 1990

A third, somewhat different system described was the 'discomat', which was used primarily for weld inspection. The detection system containing five Hall probes was rotated on a disc at typically 50 rev s- t and the tube was magnetized transversely to the direction of the weld using a magnetizing yoke. Owston t4°] has reported on measurement of leakage flux from fatigue cracks and artificial flaws such as saw slots in mild steel. These he attempted to interpret in terms of a simple dipole model of the type described by Zatsepin and Shcherbinin. The magnetic leakage field parallel to the surface and perpendicular to the cracks was measured as a function of lift-off (ie distance from the field detector to the surface of the test material). Results indicated that the leakage field increased linearly with slot depths of up to 0.2 in ( ~ 5 ram), while the derivative d2H/dz 2, where H is the magnetic field and z is the distance from the centre of the slot measured in the surface of the specimen, was found to be proportional to 1/l 4, where I is the lift-off distance. Barton et alf4~1 investigated the flux leakage method for testing of bearings, which revealed that magnetic signatures associated with pits, voids and inclusions could be identified in the leakage fields of bearing races. Forster has also written a number of papers on the subject of flux leakage at a fairly elementary level. The testing of round billets for cracks using leakage flux probes has been reported c42]. This included descriptions of both the 'tubomat' and the 'rotomat' devices. The locations of defects identified by these automated flux leakage detectors are automatically marked for ease of identification with a paint spray. These systems were capable of inspecting 12 m long billets of diameter 90-230 mm in 16 s. The most extensive review of the subject of magnetic flux leakage as an NDE tool presently available is 'NDE applications of magnetic leakage field methods' by Beissner et al t¢31. This must be considered to be the standard reference on magnetic flux leakage at this time. It contains a history of the development of the method, discusses the underlying theory, including the analysis of leakage field results and defect characterization, and finally describes a number of applications.

Leakage field calculations Once quantitative measurements of leakage fields became a routine technique, it was natural to want to interpret the signals in terms of flaw size and shape. Therefore leakage field calculations for specific flaw shapes began to be made, so that the theoretical profiles could be compared with experimental observations, with the objective of characterizing flaws from their leakage fields. Two of the most significant papers in the early development of this subject were by Shcherbinin and Zatsepin v~4'45], which were based on approximating surface defects by linear magnetic dipoles and calculating the dipole magnetic field. In this way, expressions were obtained for the normal and tangential components of the magnetic leakage field due to a defect. Zatsepin and Shcherbinin realized that the exact calculation of leakage fields arising from real defects presented an extremely complicated problem, which was intractable

NDT International April 1990

given the numerical methods and state of computer technology at that time. They therefore looked for a relatively simple problem, the leakage field of flaws which could be approximated as point, line or strip dipoles, and calculated the fields using analytical expressions. The results were then compared with observations of leakage fields due to defects, as shown in Figure 7. Notice that the horizontal component of field across the flaw leads to a unipolar response, while the normal component leads to a bipolar response. However, these early papers did not relate the leakage field to the field in the material, and therefore there were limitations on its applicability to actual measured leakage fields. Subsequent papers on leakage field calculations by Shcherbinin and Pashagin t46- 4s] were based on the same model. Experimental measurements were made on specimens of carbon steel which had artificial flaws machined in the surfaces. These defects were typically h = 0.2-3.0 mm deep, 2b = 1.0 mm wide and 21 = 1.030.0 mm long. The magnetic fields were generated using the magnetic yoke method, with a maximum magnetic field of 12 kA m-1. Measurements of the leakage field were made using a fluxgate (or 'ferroprobe') magnetometer. Field components tangential to the surface of the specimen normal to the flaw, Hx, and normal to the surface of the specimen, Hy, were measured. It was found, for example, that the relationship between the field Hy and the magnetizing field He remained almost linear, irrespective of the length of flaw, l, although the actual ratio Hr/H o increased as the flaw length increased, and in fact appeared to reach a saturation level as l --, ~ . The tangential field Hx perpendicular to the flaw was also measured. For a given flaw it was found to decay with displacement z from the centre of the flaw. Hx was also found to increase with flaw length, although this variation was dependent upon the magnetizing He. The calculations of the leakage fields by Shcherbinin and co-workers were



30 °

50 °

III C

8-c,

4

Eo~ ~

3

"'a 'l'b 2'

-~go 2 ,g~ I

o °1

c c--

3--

°.-~

2

~_,

-

C

J llJ -I0

d

e

f

F I I +10

11 ~ 111 ,10 -10 +10 -I0 Distance from crack (turn)

Fig. 7 Calculated leakage field due to a flat-bottomed flaw using the dipole model: ( a ), (b) and (c) are horizontal field components; (d), (e) and (f) are vertical field components. The slot is of length 4 mm, width 0.4 mm and depth 2 mm. In (a) and (d) the slot is normal to the surface, in (b) and (e) it is at 30 ° from the normal and in (c) and (f) it is at 50 ° from the normal. After Shcherbinin and Zatsepin E4sl

87

analogous to the fringing field calculations for idealized magnetic recording heads by Karlquist [49j. Significant progress in the calculation of leakage fields was made subsequently by Hwang and Lord ES°J using finite element methods. This was the first attempt to use numerical methods to find exact solutions to the field caused by defects. It represented a real breakthrough in the development of the subject because it enabled the leakage field to be calculated from the existing field and permeability in the bulk of the material, and it represents a landmark in the calculation of leakage fields. Some results of their calculations are shown in Figure 8. The earlier work of Zatsepin and Shcherbinin, while commendable, was not easily adaptable to the range of shapes of defects encountered in practice. The leakage field profiles obtained by Hwang and Lord for the case of a simple rectangular slot were in excellent agreement with observation. This paper was therefore instrumental in demonstrating how the finite element technique could be used for modelling fields of defects. It was clear from the work that the finite element method was sufficiently flexible that its successful application in the case of a simple slot defect indicated its likely successful application in the case of more complex defects an extension that the Zatsepin-Shcherbinin model was not capable of.

A

B

This was followed by a series of papers of which the most significant were by Lord and Hwang ts 1]and Lord et al I521. Lord and Hwang t51J extended the application of the finite element method to a variety of more complicated flaw shapes. It was deduced from this that the finite element method provided the possibility of defect characterization from the leakage field profile. It was found, for example, that the peak-to-peak value of the leakage flux BN increased with increasing flaw depth, while the separation between the peaks depended on flaw width. These results were in agreement with experimental observation and indicated the potential benefits of finite element techniques for interpreting leakage flux measurements with the objective of characterizing the defects. Lord et a1152] have remarked that the cornerstone of an approach to the application of magnetic flux leakage techniques to NDT is the development of an adequate mathematical model for magnetic field/defect interactions. It might also be added that modelling of the (B, H) or hysteresis characteristics in ferromagnetic materials adds another dimension to this problem, since even if the internal magnetic field is known there are a range of possible values of the flux density inside the material. These different possible values of B will certainly affect the leakage flux for a given type of defect with a given

C

-0.4

i--

-0.4 0.4

-- 0.4

Fig. 8 Calculated leakage field profiles due to flaws using finite element techniques (after Lord Cs3]). ( a ) B T and B N are respectively the tangential and normal components of the leakage fields across the slots shown. ( b ) Finite element calculation of the field in and around a rectangular slot in a material as a result of passing an electrical current d o w n the conductor (in this case into the plane of the paper)

88

b

NDT International April 1990

magnetizing field Ho inside the material. Lord et al concluded that the complex defect geometries, together with the non-linear magnetization characteristics of ferromagnetic steels, make closed-form or analytical solutions of magnetic field/defect interactions virtually impossible. However, they were able to show a number of examples of successful application of finite element modelling and to conclude optimistically about the potential for defect characterization for nondestructive testing. Lordt531 has given a review of the application of the finite element numerical method for calculation of leakage fields arising from magnetic field/defect interactions. In this he has indicated that much progress has been made in theoretical modelling of leakage field signatures using numerical methods, but that there are many complex problems still to be solved. Perhaps the most significant of these is taking into account the hysteresis in (B, H) characteristics of ferromagnetic materials before applying the finite element or other numerical calculation of the leakage field. The work of Lord has firmly established the use of numerical methods, such as finite element calculations, as the technique with the most promise for characterization of defects from leakage flux measurements. This has led to much interest in the area of numerical modelling of leakage fields, eg the recent work of Atherton and co.workerstS4- sr] and Bruda~ 57]. However, it was realized that three-dimensional finite element calculations are ultimately desirable for more precise characterization of real defects. An analytic solution for the leakage field of surfacebreaking cracks has recently been presented by Edwards and Palmer tsal in which the crack is approximated as a semi-elliptic slot in the material. The advantages of an analytic expression are that the fields due to defects can be rapidly calculated, and in addition the equations can be differentiated to find the forces on magnetic particles. From these results Edwards and Palmer calculate the magnetic field strength H needed to detect 1 #m and 10 /tm wide slots for a range of slot depths and permeabilities. They conclude that fields in the range 102-103 A m -1 are required for crack detection, and these are in agreement with those used in practice, eg BS 6072tl°] which recommends a magnetic induction of 0.72 T, corresponding to a field of 5700 A m - 1 in a steel of relative permeability 100. Reviews of the subject of magnetic leakage field calculations and the interpretation of experimental measurements have been given by Dobmann tsg] and Holler and Dobmann tr°]. Dobmann tsg] has discussed the problems of both detection and sizing of defects and has attempted to relate these to theoretical model predictions. Theoretical work on flux leakage has lagged considerably behind experimental development. Dobmann and Holler tr°] have reviewed the theoretical modelling of the effects of various flaws on the leakage flux, and Forster t61] has attempted to correlate observed magnetic flux leakage measurements with expectations based on finite element model calculations. His results showed serious discrepancies. This has made it difficult to characterize flaws quantitatively in some cases, although qualitatively the explanations are relatively simple and have been very successful.

NDT International April 1990

Eddy current inspection Eddy current methods for nondestructive evaluation are not strictly magnetic methods as such. That is, they do not depend for their validity on any inherent magnetic properties of the material under test. In fact, they can be applied to any conducting material. Furthermore, the literature for eddy current techniques is more extensive than that of all the other magnetic methods combined and so it would not be possible to give a comprehensive review of the subject in this paper. Nevertheless, in the interests of completeness, eddy currents do deserve mention since they are used on magnetic materials. The eddy current inspection method depends on the change in inductance of a search coil in the vicinity of a conducting test specimen caused by the generation of electrical currents in the test specimen when it is subjected to a time-varying magnetic field (Figure 9). The response is usually monitored in the form of a complex impedance plane map. Eddy currents can be used for the detection of cracks and other defects, because the defects interrupt the flow of the eddy currents generated in the material. This results in a different complex impedance of the eddy current pick-up coil when it is positioned over the flaw compared with when it is positioned over an undamaged region of the material. Eddy currents can also be used for checking thickness of coatings, determining permeability and conductivity, evaluating changes in heat treatment and microstructure, and estimating tensile strength, chemical composition and ductility. However, whereas the interpretation of results in non-magnetic materials is relatively straightforward, in ferromagnetic materials it is more difficult because the eddy current response depends on permeability. In ferromagnetic materials such as steels the permeability varies in a complicated way with the generating field. Much of the early work on development of eddy current techniques was due to Forster t62-651. A survey of the field until 1970 was given by Libby t66] and more recently by Lord [67].

Applications of eddy current inspection Application of eddy current techniques to magnetic materials by Vroman tra] has shown that the results are Time -varying magnetic field H(t) Time - dependent current I(t)

-T---" Vi

_Z__,

c/

"

l

Eddy currents generated in solid

Fig. 9 Generation of eddy currents in a conducting material by a time-varying magnetic field

89

easier to interpret if the material is subjected to a saturating DC field at the same time as the AC field which generates the eddy currents. This ensures that the prior state of magnetization of the material no longer affects the observed results, while also preventing large changes in permeability. Cecco and Bax [69] saturated the magnetization within their steam generator tubing while scanning for defects. In this way they reported that they obtained improved sensitivity over earlier attempts to use eddy currents for ferromagnetic tubes, which had been hampered by inherent 'magnetic noise'. Deeds and Dodd [7°] have reported on detection of defects such as cracks, wall thinning or holes in steam generator tubing using eddy currents. Dodd and Simpson t711 developed a low-frequency eddy current system for accurate determination of small changes in permeability of weakly magnetic materials, which was used to evaluate the fabrication of austenitic stainless steels. This was able to determine the amount of cold working in components and to determine the amount of 6-ferrite in welds, which reduces the incidence of hot cracking in the welds. Detection of the depth of case hardening in steels by eddy current inspection has been reported by Kuznetsov and Skripova t~2]. Clark and Junker t~31 have established the feasibility of an eddy current NDT approach for the detection of temper embrittlement in low-alloy steels, which was known to be difficult to detect by other methods. Eddy currents have also been used for mapping localized changes in residual stress using automated scanning equipment by Clark and Taszarek t~41. However, they concluded that the method was unable to discriminate between tensile and compressive residual stresses - only the absolute magnitude of stress could be ascertained. Lord and Palanisamy t75] have also used eddy currents for inspection of steam generator tubing and modelled the results using finite element techniques. T h e r e m o t e field electromagnetic technique

inspection

The remote field electromagnetic inspection technique is based on the diffusion of electromagnetic energy through a pipe wall. This can be used for the detection of corrosion or other forms of wall thinning in pipes and oil well castings. The method was developed in the 1950s and early 1960s, but it is only in recent years that it has suddenly received great attention as an NDE technique. One of the earliest descriptions of the method was by Schmidd TM, who used it for in situ detection of external casing corrosion in down-hole inspection in oil wells. This was an important breakthrough because there were no other techniques available at that time for detection of external corrosion. The advantages of the method over conventional eddy current and ultrasonics inspection, which can also be used for measuring wall thickness, include full 360 ° scanning of the pipe, rapid logging speeds and its insensitivity to dirt or scale on the pipe. Schmidt t771has reviewed the remote field electromagnetic inspection technique. He has shown that the development of improved spatial resolution of these instruments has allowed isolated pits and cracks in the pipe wall to be resolved, a result not possible with alternative techniques under the conditions encountered in down-hole inspection.

90

The method has been used for detection and classification of stress corrosion cracking. The advantage of the remote field technique is that it detects only a flux which has penetrated and been transmitted through the pipe wall. Even though both the transmitter and receiver coils are located within the pipe, there is very little direct coupling between them. Therefore the detected signal contains information about the pipe wall thickness. The variation of the detected signal with distance between exciter and receiver coils is shown in Figure 10. The technique is equally sensitive to both interior and exterior metal loss, and the observed phase lag was found to be linear with wall thickness, which is a very useful result. Finally, the problems that are normally encountered with lift-off in eddy current inspection are less evident in the remote field technique. This method has been investigated recently by Atherton and Sullivan tTs] for inspecting zirconium-2.5 % niobium nuclear reactor pressure tubes, which are non-magnetic, for the presence of defects. In this they operated the detection coil at a distance of one pipe diameter from the transmitter coil, as shown in Figure 11. They have also indicated that their results are consistent with Schmidt's original suggestion that the Signals are caused by a diffusion process through the wall close to the transmitter coil, followed by propagation along the outside of the tube, and then diffusion back through the pipe wall. Subsequently, finite element calculations were applied to model the propagation of the electromagnetic signals in the remote field eddy current technique/79]. The results of these calculations confirmed the mode of propagation originally suggested. A review of the history of eddy current inspection of steel tubing has been given by Black [8°], while Dorofeev roll has surveyed the use of eddy currents for evaluation of quality of steel components. Two elementary reviews of eddy current methods have appeared in the last few years, by Franklin ts2~ and by McMaster m3].

10-I

' I ' I ' I ' I ' I ' I

IO-~ ~ i

'

I

'

~mol~tu~

I 360

270

Eo ,6'

=so ~o \

=¢J 16s

| ~

Phase-

~ OUter Iv -

\ I

~"..........~.WOll

inner

o

[K_......I~ ~ Id e . IC~'

Direct coupling zone ,

0

I I

9o

Remote field zone ,

II P

,

I 5

,

I 4

,

[ 5

,

I 6

,

I 7

,

I '0 8

Pipe diameter from exciter coil Fig. 1 0 V a r i a t i o n o f phase and amplitude of detected signal as a f u n c t i o n of distance between exciter and receiver coils within the pipeline. ( A f t e r S c h m i d t [77])

NDT International April 1990

Pipe well

Energy flow path

Pick-up coil

15 16 17 18

/ Drive rod

Transmitter coil

19

Wheel support

Fig. 1 1 Arrangement for the remote field electromagnetic inspection of pipes as described by Atherton and Sullivan [78]

Conclusions Three major classes of technique for detection and characterization of flaws and defects in ferromagnetic materials have been discussed. These are magnetic particle inspection, magnetic flux leakage and eddy current or electromagnetic inspection. The relative advantages and disadvantages of each technique have been discussed, and a wide survey of existing literature has been given. The objective of this review has been to provide an introduction to the various magnetic methods for nondestructive evaluation, and in conjunction with the preceding pape rtl] it gives a comprehensive review of the field. It is not possible in a paper such as this to discuss each method in detail, nor is it even desirable. The references given here do provide access to the specialized literature of each method and further details can be obtained from these.

20 21 22 23 24 25 26 27

28 29

Acknowledgement

30

This work was sponsored by the Center for NDE at Iowa State University and was performed at the Ames Laboratory. Ames Laboratory is operated for the US Department of Energy by Iowa State University under Contract W-7405-ENG-82.

31

References

33

1 2 3 4 5 6 7 8 9 10 11 12 13 14

Jiles, D.C. 'Review of magnetic methods for N D E ' N D T International 21 (1988) p 311 Saxby, S.M. 'Magnetic testing of iron' Engineering 5 (1868) p 297 Hoke, W. in Principles of Magnetic Particle Testing ed C.E. Betz, Magnaflux Corporation, Chicago (1967) p 48 deForest, A.V. 'Magnetic testing of iron and steel' Iron & Steel Eng 9 (1932) p 170 Doane, F.B. 'Magnaflux inspection for cracks and seams' Iron Age (September 1933) MagnaBax Corporation 300 W Lawrence Avenue, Chicago, IL 60656, USA Fo~ter, F. 'Developments in magnetography of tubes and tube welds' Nondestructive Testing g (1975) p 304 Gregory, C.A., Holmes, V.L and Roehr~ R.J. 'Approaches to verification and solution of magnetic particle inspection problems' Mater Eval 30 (1972) p 219 Mama, G.M. 'Finding the optimum conditions for weld testing by magnetic particles' N D T International 9 (1976) p 16 British Standards Institution 'Method for magnetic particle flaw detection' British Standard 6072 ( 1981 ) Raine, G.A., Robinson, A.N. and Nolan, P. 'Magnetic particle inspection of pressure vessels and pipelines and associated field strength measurements' Br J N D T 26 (1984) p 420 Edwards, C. and Palmer, S.B. 'An analysis of the threading bar method of magnetic particle flaw detection' ND Tlnternational 14 (1981) p 177 Edwards, C. and Palmer, S.B. 'The prod magnetization method of magnetic particle inspection' Br J N D T 25 (1983) p 305 Oehl, C.L. and Swartzeadmber, L J . 'On the optimum applied field for magnetic particle inspection using direct current' J NDE 3 (1982) p 125

NDT International April 1990

32

34 35

36 37 38

39 40 41 42 43 44

Cr'lb~"Y;F, 'Automatic crack detection with computer vision and pattern recognition of magnetic particle indications' Mater Eval 42 (1984) p 1506 Bezer, H.J. 'Magnetic methods of nondestructive testing (Part 1)' Br J N D T 6 (1964) p 85 Bezer, H.J. 'Magnetic methods of nondestructive testing (Part 2)' Br J N D T 6 (1964) p 109 Be=r, H.J. 'Magnetic particle inspection techniques and their application in the U.K.' Br J N D T 13 (1971) p 2 Duna, F.W. 'Magnetic particle inspection fundamentals' Mater Eval 35 (1977) p 42 Betz, C.E. Principles of Magnetic Particle Testing Magnaflux Corporation, Chicago (1966) Stumm, W. 'Magnetic stray flux techniques in nondestructive testing - theory, applications, new developments' Br J NDT 21 (1979) p 193 Stumm, W. 'Inservice nondestructive inspection of heavy loaded structures, in particular underwater structures, with leakage flux methods' Br J N D T 25 (1983) p 124 Znschlag, T. 'Method and apparatus for testing rails or the like' US Patent 1,896,737 (1933) Hastings, C.H. 'Disclosure of principles and details of a new method for the detection of flaws in ferromagnetic materials' WAL TR 732/114 Army Materials and Mechanics Research Center (1946) Hastings, C.H. 'A new type of magnetic flaw detector' A S T M Proc 47 (1947) p 651 Bainton, K.F. 'Characterizing defects by determining magnetic leakage fields' N D T International 10 (1977) p 253 Teller, C.M., Barton, J.R., Matzkanin, G.A., Knsenberger, F.N. and Beissner, R.E. 'Correlations between advanced NDE methods and fracture mechanics parameters' J Eng Mater & Technol 102 (1980) p 50 Atherton, D.L, Coathup, LW., Jiles, D.C., Longo, L., Welbourn, C. and Teitsma, A.l'Stress induced magnetization changes of steel pipes - laboratory tests'/IEEE Trans. Magn MAG-19 (1983) p 1564 Atherton, D . L and Teitsma, A. 'Detection of anomalous stresses in gas pipelines by magnetometer survey' J. Appl. Phys. 53 (1982) p 8130 Atherton, D.L., Welbourn, C., Jiles, D.C., Reynolds, L. and Scott Thomas, J. 'Stress induced magnetization changes of steel pipes - laboratory tests (Part 2)' IEEE Trans. Magn MAG-20 (1984) p 2129 Atherton, D.L. and Quek, E. 'Distinction between near and far side corrosion pit signals using magnetic leakage flux detectors Can. Electr. Eng. J. 13 (1988) p 27 Atherton, D.L. 'Stress shadow magnetic inspection technique for far side anomalies in steel pipe' N D T International 16 (1983) p 145 Kalileev, P.A. and Grigorev, P.A. "Methods of testing the condition of underground pipes in main pipelines' Soy J N D T 10 (1974) p 438 Grigorev, P.A., Fridman, LA. and KImlileev, P.A. 'A magnetizing flaw detection system for the inspection of underground pipelines' Soy J NDT 12 (1976) p 351 Pnshagin, A.I., Sheherbinin, V.E.,! Banklevsimys, N.P., Filippov, B.A. and Marulin, A.P. 'Effect of the magnetizing method on the detectability of defects in welded joints in electric welded pipes' Soy J NDT 20 (1984) p 753 Ferster, F. 'The magnetic leakage field method of nondestructive testing (Part 1)' Mater Eval 43 (1985) p 1154 Forster, F. 'The magnetic leakage field method of nondestructive testing (Part 2)' Mater Eval 43 (1985) p 1398 Forster, F. 'Nondestructive inspection by the method of magnetic leakage fields. Theoretical and experimental foundations of the detection of surface cracks of finite and infinite depth' Soy J N D T 18 (1982) p 841 Stumm, W. 'Tube testing by electromagnetic NDT methods' Nondestructive Testing 7 (1974) p 251 Owston, C.N. 'The magnetic flux leakage technique of nondestructive testing' Br J N D T 16 (1974) p 162 Barton, J.R., Lankford, J. and Hampton, P.L. 'Advanced nondestructive testing methods for bearing inspection' Soc Auto Eng Trans 81 (1972) p 681 Forster, F. 'Nondestructive inspection of tubing and round billets by means of leakage flux probes' Br J N D T 19 (1977) p 26 Beissner, R.E., Matzlumin, G.A. and Teller, C.M. 'NDE applications of magnetic leakage field methods' S W R I Report NTIAC-80-1 (1980) Zatsepin, N.N. and Sheherbieia, V.E. 'Calculation of the magnetic field of surface defects. I. Field topography of defect models' Soy J N D T 2 (October 1966) p 50

91

45

46 47 48 49 50 51 52 53 54 55 56 57 58 59

60 61 62 63 64

Shcherbinin, V.E. and Zatsepin, N.N. 'Calculation of the magnetostatic field of surface defects, lI. Experimental verification of the principal theoretical relationships' Soy J NDT 2 (October 1966) p 59 Shcherbinin, V,E. and Pashagin, A.I. 'Influence of the extension of a defect on the magnitude of its magnetic field' Soy J NDT 8 (1972) p 441 Shcherb/nin, V.E. and Pashagin, A.l."On the volume polarization of cracks' Soy J NDT 10 (1974) p 460 Shcherbinin, V.E. and Pashagin, A.I. 'Fields of defects on the inner and outer surfaces of a tube during circular magnetization' Soy J N D T 8 (1972) p 134 Karkluist, O. 'Calculation of the magnetic field in the ferromagnetic layer of a magnetic drum' Trans R lnst Technol, Stockholm ~6 (1954) p 3 Hwang, J.H. and Lord, W. 'Finite element modelling of magnetic field-defect interactions' J Test & Eval 3 (1975) p 21 Lord, W. and Hwang, J.H. 'Defect characterization from magnetic leakage fields' Br J NDT 19 (1977) p 14 Lord, W., Bridges, J.M., Yen, W. and Palanisamy, R. 'Residual and active leakage fields around defects in ferromagnetic materials' Mater Eval 36 (1978) p 47 Lord, W, 'Applications of numerical field modelling to electromagnetic methods of nondestructive testing' IEEE Trans Magn MAG-19 (1983) p 2437 Atherton, D.L and Daly, M.G. "Finite element calculation of magnetic flux leakage detector signals' NDT International 20 (1987) p 235 Atherton,D . L and Czura, W. 'Finite element calculations on the effects of permeability variation on magnetic flux leakage signals' NDT International 20 (1987) p 239 Atherton, D . L 'Finite element calculations and computer measurements of magnetic flux leakage patterns for pits' Br J NDT 30 (1988) p 159 Brndar, B. 'Magnetic leakage fields calculated by the method of finite differences' NDT International 18 (1985) p 353 Edwards, C. and Palmer, S.B. 'The magnetic leakage field of surface breaking cracks' J Phys D: Appl Phys 19 (1986) p 657 Dohmann, G. 'Magnetic leakage flux techniques in NDT: a state of the art survey of the capabilities for defect detection and sizing' in Electromagnetic Methods of NDT ed W. Lord, Gordon and Breach, New York (1985) p 71 Holler, P. and Dobmann, G. 'Physical analysis methods of magnetic flux leakage' in Research Techniques in NDT vol IV, ed R.S. Sharpe, Academic Press, New York (1980) p 39 Forster, F. 'New findings in the fields of nondestructive magnetic leakage field inspection' NDT International 19 (1986) p 3 Forster, F. 'Theoretical and experimental foundations of nondestructive evaluation with eddy currents. I" Z Metallk 43 (1952) p 163 Forster, F. 'Theoretical and experimental foundations of nondestructive evaluation with eddy currents. IV' Z Metallk 45 (1954) p 180 Forster, F. and Ikeitfeld, H. 'Theoretical and experimental foundations of nondestructive evaluation with eddy currents. V' Z Metallk 45 (1954) p 188

65 66 67 68 69 70 71 72 73 74 75 76 77 78 79 80 81 82 83

Forster, F. 'Theoretical and experimental foundations of nondestructive evaluation with eddy currents. VII' Z Metallk 45 (1954) p 221 Lihhy, H.L. Introduction to Electromagnetic Nondestructive Test Methods Wiley, New York ( 1971 ) Lord, W. Electromagnetic Methods of Nondestructive Testing Gordon and Breach, New York (1985) Vroman, J. 'The influence of magnetic properties on eddy current testing of a tube' Br J NDT 23 (1981) p 307 Ceeeo, V.S. and Bax, C.R. 'Eddy current in-situ inspection of ferromagnetic monal tubes' Mater Eval 33 (1975) p 1 Deeds, W.E. and Dodd, C.V. 'Eddy current inspection of steam generator tubing' in Electromagnetic Methods of Nondestructive Testing ed W. Lord, Gordon and Breach, New York (1985) Dodd, C.V. and Simpson, W.A. 'Measurement of small magnetic permeability changes by eddy current techniques' Mater Eval 29 (1971) p 217 Kuznetsov, I.A. and Skripova, N.M. 'Nondestructive measurement of the depth and hardness of the carburized case on parts of 12KhN3A and 12Kh2N4A steels' Soy J NDT 19 (1983) p 410 Clark, W.G. and Junker, W.R. 'Problems in the eddy current characterization of temper embrittlement' Mater Eval 43 (1985) p 1546 Clark, W.G. and Taszarek, B.J. 'Stress mapping with eddy currents' Mater Eval 42 (1984) p 1272 Lord, W. and Palanisamy, R. 'Magnetic probe inspection of steam generator tubing' Mater Eval 38 (1980) p 38 Schmidt, T.R. 'The casing inspection tool - an instrument for the in situ detection of external casing corrosion in oil wells' Corrosion 17 (1961) p 81 Schmidt, T.R. 'The remote field eddy current inspection technique' Mater Eval 42 (1984) p 225 Atherton, D.L. and Sullivan, S. 'The remote-field, through-wall electromagnetic inspection technique for pressure tubes' Mater Eval 44 (1986) p 1544 Atherton, D.L., Szlamar, B. and Sullivan, S. 'The application of finite element calculations to the remote field inspection technique' Mater Eval 45 (1987) p 1083 Black, W.A. 'Eddy current testing of steel tubing' Mater Eval 43 (1985) p 1490 Dorofeev, A,L. 'Use of the electromagnetic method of inspection of the quality of parts in machine building' Soy J NDT 15 (1979) p 183 Franklin, E.N. 'Eddy current inspection' Mater Eval 40 (1982) p 1008 MeMaster, R.C. 'The present and future of eddy current testing' Mater Eval 43 (1985) p 1512

Author The author is in the Center for Nondestructive Evaluation and the Department of Material Science and Engineering, Iowa State University, Ames, Iowa 50011, USA.

Paper received 19 May 1 989

92

NDT International April 1990