Effects of extrusion parameters on tensile properties of magnesium alloy tubes fabricated via hydrostatic extrusion integrated with circular ECAP Renshu Yuan, Zhilin Wu, Hongming Cai, Lei Zhao, Xinping Zhang PII: DOI: Reference:
S0264-1275(16)30436-1 doi: 10.1016/j.matdes.2016.03.141 JMADE 1619
To appear in: Received date: Revised date: Accepted date:
30 January 2016 19 March 2016 29 March 2016
Please cite this article as: Renshu Yuan, Zhilin Wu, Hongming Cai, Lei Zhao, Xinping Zhang, Effects of extrusion parameters on tensile properties of magnesium alloy tubes fabricated via hydrostatic extrusion integrated with circular ECAP, (2016), doi: 10.1016/j.matdes.2016.03.141
This is a PDF file of an unedited manuscript that has been accepted for publication. As a service to our customers we are providing this early version of the manuscript. The manuscript will undergo copyediting, typesetting, and review of the resulting proof before it is published in its final form. Please note that during the production process errors may be discovered which could affect the content, and all legal disclaimers that apply to the journal pertain.
ACCEPTED MANUSCRIPT Effects of extrusion parameters on tensile properties of magnesium alloy tubes fabricated via hydrostatic extrusion integrated with circular ECAP
School of Mechanical Engineering, Nanjing University of Science and Technology,
IP
a)
T
Renshu Yuan a), Zhilin Wu a,b), Hongming Cai a,b), Lei Zhao a,b), Xinping Zhang c,*)
Nanjing, 210094, China
Institute of Science and Technology, Nanjing University of Science and Technology,
SC R
b)
Nanjing, 210094, China c)
School of Material Science and Engineering, Nanjing University of Science and
NU
Technology, Nanjing, 210094, China
MA
Abstract: To meet the need for high strength tubes for various industrial applications, a new method, known as hydrostatic extrusion integrated with circular equal channel angular pressing (HECCAP), was proposed for the fabrication of AZ80 magnesium
D
alloy tubes. Small diameter billets could be extruded into tubes of larger diameters
TE
using this method. The effects of the extrusion ratio (ER) and the conical mandrel angle (CMA) on the microstructure and tensile properties of the AZ80 magnesium alloy tube
CE P
were investigated. The HECCAP-treated alloys exhibited a partial dynamically recrystallized microstructure. More shear zones formed inside of these grains, and a higher recrystallization grain volume fraction were presented in the alloy after HECCAP treatment with a larger ER or CMA values. The tensile yield strength,
AC
ultimate tensile strength, and elongation percent increased as ER and CMA also increase. The highest ultimate tensile strength, tensile yield strength and elongation were 335 MPa, 308 MPa, and 7.2 %, respectively, at an ER of 2.77 and CMA of 120°. A formula was proposed to calculate the total generated plastic strain after HECCAP, which increased with increasing ER and CMA.
Key words: AZ80 magnesium alloy; Warm-hydrostatic extrusion; Microstructure; Mechanical properties; Extrusion ratio; Conical mandrel angle Corresponding author: X.P. Zhang. Tel. / fax: + 86 25 84303983. E-mail address:
[email protected] (X.P. Zhang). Complete postal address: School of Materials Science and Engineering, Nanjing University of Science and Technology, Xiaolingwei 200, Nanjing 210094, China 1
ACCEPTED MANUSCRIPT 1. Introduction Severe plastic deformation (SPD) techniques can improve the material properties of alloys by refining their grain structure. Such methods are attractive as ultra-fine grained
T
(UFG) materials have been shown to exhibit outstanding material properties, such as
IP
high strength [1]. Most SPD methods, such as equal channel angular pressing (ECAP), high-pressure torsion, and accumulative roll bonding, are suitable for various
SC R
geometries, including bars, rods, plates, and sheets. Despite the need for high strength tubes for various industrial applications, little effort has been made to produce tubular parts using SPD methods.
NU
Magnesium alloys are increasingly used in the automotive and aerospace industries due to their low density and high specific strength [2]. ECAP is deemed to be the most
MA
efficient SPD technique for refining the microstructure. When the ECAP technique is integrated into a hydrostatic extrusion die for tubes, the extruded parts will have UFG properties. The high hydrostatic pressure during extrusion will reduce crack defect
D
induced by ECAP. These benefits make such a process attractive for commercial use.
TE
In the present work, a new method, named as hydrostatic extrusion integrated with circular equal channel angular pressing (HECCAP) method, was proposed to fabricate
CE P
AZ80 magnesium alloy tubes. Effects of the extrusion ratio (ER) and conical mandrel angle (CMA) on microstructure and tensile properties of AZ80 magnesium alloy tube were investigated.
2. Materials and methods
AC
2.1 Material
Direct chill (DC) cast alloy with an average composition of Mg-8.5% Al-0.49% Zn-0.21% Mn (AZ80) was received in the form of cylindrical ingots with dimensions of Ø 70 mm × 400 mm. 2.2 Hydrostatic extrusion experiment A schematic of the HECCAP extrusion die is shown in Fig. 1. The diameter of the billet is the same as the maximum outer diameter of the mould core. There were two ECAP channels between the extrusion container and the mould core. The billets were extruded in two passes with a channel angle (φ). The corner angles (ψ) of these passes were 0°. The working procedure of the hydrostatic extrusion starts by lading a billet into the container, then sealing the container with the ram and filling it with castor oil, after which the ram is then advanced into the container. This pressurizes the chamber forcing the billet through the die. The extrusion speed is approximately 0.2 mm/s. 2
ACCEPTED MANUSCRIPT As informed by previous research on the effects of heat treatment on microstructures and mechanical properties of Mg AZ80 alloys [3-6], the AZ80 alloy ingots with a diameter of 70 mm were homogenized at 415 °C for 32 h, and then machined into
T
billets with a diameter of 60 mm. These billets were heated in a furnace at 290 °C for 1
IP
h and then extruded to tubes with an outer diameter of 70 mm and an inner diameter dependent on the ER.
SC R
Due to the limitations of the sealing material, the pre-heat temperature of the extrusion container was set to 220 °C. Due to limitations in the extrusion force of the hydrostatic extruder, the ERs were set as 1.25, 1.92 and 2.77, while the conical mandrel angle
2.3 Tensile test at room temperature
NU
CMA values were fixed at 105° and 120°. Experiments were performed in triplicate.
MA
Dog-bone-shaped flat specimens with a 6 mm gauge length and a 2 mm gauge width were used in the tensile tests. The tensile test specimens were sectioned along the extrusion axis. The dimensions of the specimens and the test methods used in this study
D
are identical to those documented previously [7, 8]. Placements of the tensile specimen
TE
and microstructure specimen are shown in Fig. 2. Tensile yield strength was determined by the offset method as described in ASTM: E9-89a, with an offset of 0.2%.
CE P
2.4 Microstructural characterization N side (radial direction) and S side (extrusion direction) samples (see Fig. 2) were prepared for microscopy analysis by polishing them with various grades of SiC paper (with increasing fineness) and with 1 µm diamond paste in the last step. The samples
AC
were then ultrasonically cleaned in pure ethanol. In order to make the grain structure easily visible, the polished samples were etched in a solution of 100 ml ethanol, 6 g picric acid, 5 ml acetic acid, and 10 ml water. Microstructural and composition characterization were carried out using optical microscopy (OM), scanning electron microscopy (SEM, FEI Quanta 250 FEG) and energy disperse spectroscopy (EDS). The phases of the alloy were confirmed by X-ray diffractometry (XRD, Bruker D8 X) using Cu Kα radiation. 3. Results and Discussion 3.1 Homogenized and HECCAP-treated microstructures An example of an AZ80 tube prepared using the HECCAP method is shown in Fig. 3. It can be seen that the resulting surface is quite smooth (the average roughness Ra ≤ 3.0 μm). After cutting off the stub bar, the variation in the wall thickness over the length of the tube was ≤0.3 mm. 3
ACCEPTED MANUSCRIPT The radial-forward extrusion method is a method of fabricated a larger diameter tube from a small diameter billet [9-10]. In this work, small diameter billets were extruded into tubes of larger diameters using the HECCAP method. The major difference
T
between the radial-forward extrusion method and the HECCAP method is back
IP
pressure. Back pressure (BP) is generated during the HECCAP due to castor oil while there is no back pressure during the radial-forward extrusion. The application of a BP
SC R
ensures the homogeneity of the workpiece processed and leads to an increased rate of continuous dynamic recrystallization (CDRX) [11]. Due to the hydrostatic pressure conditions, the BP is advantageously able to reduce or completely eliminate dead zones,
NU
which contributes to an increase in the magnitude and homogeneity of the imposed strain along the cross section of the deformed workpiece. Additional benefits include
MA
significant reductions in tensile stress areas, which can initiate the development of cracks or fractures [12]. Hence, the HECCAP method can improve the homogeneity of the workpiece, refine the microstructure of the workpiece, and decrease the defects.
D
Typical microstructures and XRD results of the homogenized AZ80 Mg alloy are
TE
shown in Fig. 4. The grey features in Fig. 4 (a) and the black features in Figs. 4 (b)-(c) was α phase Mg. Eutectic structures (formed during non-equilibrium freezing) were
CE P
present on the boundary of this phase. The black features in Fig. 4 (a) and the grey features in Figs. 4 (b)-(c) correspond to Mg17Al12 (II), which had a lamellar structure. The small undissolved particles located in the grains were Mg17Al12. It was verified by the EDS results, as listed in Table 1. The mean grain size and the non-base matrix
AC
phase (eutectic structure, Mg17Al12 (II), and Mg17Al12) contents of the homogenized specimen were 75 ± 8 µm and 9 ± 3%, respectively. Fig. 5 shows the microstructures of the HECCAP-treated AZ80 Mg alloy. A large amount of new fine grains appeared at the initial grain boundary, due to dynamically recrystallization. Refine eutectic and Mg17Al12(II) also appeared along the grain boundary. The AZ80 Mg alloy exhibited a partial dynamically recrystallized (DRXed) microstructure. The partial DRXed microstructure was most likely due to the relatively low extrusion temperature (290 °C) and slow extrusion speed used (approximately 0.2 mm/s), which are known to reduce the DRX fraction [13]. Furthermore, there were no bands of stringers parallel to the extrusion direction present in any specimens. The shear force appeared when the billet moved through the two ECAP channels, leading to shear zones formed inside of the grains, as shown in Fig. 5 (b). 4
ACCEPTED MANUSCRIPT Large particles (diameter > 1 µm) can act as nucleation sites for DRX during hot deformation ( also known as particle-stimulated nucleation) [14-17], and although the larger Mg17Al12 particles (2–15 µm, see Fig. 5) were partially broken during extrusion,
T
their size remains greater than 1µm, as shown in Fig. 5 (C). We therefore believe that
IP
these particles acted as heterogeneous sites for nucleation of recrystallization by generating local inhomogeneity in the strain energy during extrusion, resulting in an
SC R
increase in the DRX fraction of the HECCAP-treated alloy.
The difference between the microstructure at the N side and the S side were the DRX fraction, the grain size and shape. The DRX fraction at the S side was larger than that
NU
at the N side, while the grain size and the ratio of length to width of the grain of the former were smaller than these of the latter.
MA
3.2 Effects of extrusion ratio on the microstructure and tensile properties of HECCAP-treated AZ80 Mg alloy
Typical microstrcutures of the HECCAP-treated AZ80 Mg alloy with different ERs
D
are shown in Fig. 6. More shear zones formed inside of the grains, and a higher DRX
TE
fraction were appeared in the AZ80 Mg alloy treated using HECCAP at a larger ER value. For example, the DRX fraction increased from 43% to 50% and 75% when the
CE P
ER increased from 1.25 to 1.92 and 2.77. The expression for the volume fraction of a dynamically recrystallized grain Xd obtained by the classical treatment of grain boundary nucleation kinetics proposed by Cahn [18] is given by Equations (1) and (2):
AC
(1) (2)
where ε is the plastic strain, εp is the peak strain, a1 ,a2 , n1 are the material constants,
is strain rate, n is the stress exponent, Q is the activation energy for the deformation, R is the gas constant, 8.314 J/mol, and T is absolute temperature. As εp increases with (see Eq. (2)), it prevents the occurrence of DRX. When the extrusion speed is held constant, the strain rate increases as ER increases. Accordingly, the εp needed to cause DRX of specimens extruded at a lower ER is lower than that at a larger ER value, which prevents the occurrence of DRX when the specimen is extruded at a larger ER. However, a larger ER leads to a higher strain, which promotes DRX when the specimen is extruded at a larger ER. In addition, a larger ER 5
ACCEPTED MANUSCRIPT improves the temperature increase of the billet during HECCAP. Higher deforming temperatures reduce εp, which also promotes DRX when the specimen is extruded at a larger ER. In this work, a larger ER increases the DRX fraction.
T
The effects of ER on the tensile properties of HECCAP-treated AZ80 Mg alloy tubes
IP
are shown in Fig. 7. The tensile yield strength, ultimate tensile strength, and elongation percent all increased as ER increased. The highest ultimate tensile strength, tensile
SC R
yield strength and elongation were 335 MPa, 308 MPa, and 7.2 %, respectively, at an ER of 2.77 and CMA of 120 °.
The tensile properties of the HECCAP-treated AZ80 Mg alloy tubes were not lower
NU
than those of the SPDed AZ80 Mg alloy. For example, Sepahi-Boroujeni et al the as-cast through the expansion equal channel angular extrusion (Exp-ECAE) operation.
MA
The maximal ultimate tensile strength is 298 MPa [19]. Chen et al reported the UTS, YS and elongation to fracture of the repetitive upsetting-extrusion AZ80 magnesium alloy are 337 MPa, 246MPa and 24.6%, respectively [20]. Cao et al reported the
D
ultimate tensile strength and elongation of the hot flow formed AZ80 magnesium alloy
TE
were 308 MPa and 9.8%, respectively [21]. The tensile strength of the AZ80 Mg alloy could be attributed to the combined effects of
CE P
several strengthening mechanisms: (1) grain boundary strengthening by ultra-fine fully DRXed grains, (2) strain hardening, (3) precipitation strengthening by fine Mg17Al12 precipitates, and (4) solid-solution strengthening by dissolved Zn. The tensile -
AC
elongation of extruded Mg alloys is strongly related to their DRX fraction [22]; that is, -
-
{1011} contraction and {1011}-{1012} double twinning are more easily generated in large unDRXed grains during tensile deformation along the elongation direction at room temperature, which in turn provides initiation sites for micro-cracking that degrade the ductility [23-25]. Thus, the higher tensile elongation of the AZ80 Mg HECCAP-treated at a larger ER was most likely a result of its greater DRX fraction, or more specifically the relative lack of large unDRXed grains. In addition, a larger ER allowed for greater strain hardening, which also improved the tensile strength of AZ80 Mg treated using HECCAP at a larger ER. 3.3 Effects of conical mandrel angle on the microstructural and tensile properties of HECCAP-treated AZ80 Mg alloys Typical microstrcutures of AZ80 Mg alloy HECCAP-treated with different CMAs are shown in Fig. 8. More shear zones formed inside of the grains and a higher DRX 6
ACCEPTED MANUSCRIPT fraction appeared in the AZ80 Mg alloy HECCAP-treated with a larger CMA. For example, the DRX fraction increased from 31 % to 43 % when CMA increased from 105° to 120°.
T
The effects of CMA on the tensile properties of HECCAP-treated AZ80 Mg alloy
elongation percent increased as the CMA was increased.
IP
tubes are shown in Fig. 9. The tensile yield strength, ultimate tensile strength, and
SC R
The flow pattern and strain-stress states of HECCAP are different from those of conventional ECAP. In conventional ECAP, the strain state can be considered as simple shear, while in HECCAP there are some additional radial and circumferential resulting from
NU
tensile and compressive strains. To calculate the accumulated strain
conventional ECAP with channel angles φ and corner angles ψ, the following Equation
MA
[3] can be used:
(3)
D
During the first pass, the flow pattern and the strain-stress state of the material near the
TE
container wall is different from that of the material near the mould core. Hence, the average accumulated strain during the first pass is set as the product of λ and the
CE P
corresponding value of conventional ECAP. λ is a function of CMA and φ and 0 < λ < 1. It should be noted that the method for accurately determining a value for λ merits further investigation.
applied to the alloy during HECCAP processing can be
AC
The total accumulated strain
calculated using Equation (4), derived from common engineering plasticity formulae and the geometry values shown in Fig. 1: (4)
In this work, ψ is 0°, so
can be written using Equation (5): (5)
The relationship between the CMA γ (0 < γ < π) and φ defined using Equation (6): (6) That is,
7
ACCEPTED MANUSCRIPT (7)
where 0 < γ < π/4. increased with the values of CMA and ER. As a consequence, the effects
T
Hence,
IP
of CMA on the microstructure and tensile properties were the same as those of ER. 4. Conclusions
SC R
Small diameter billets were extruded into tubes with a larger diameter using a hydrostatic extrusion process integrated with circular equal channel angular pressing method.
NU
These HECCAP-treated AZ80 alloys exhibited a partial dynamically recrystallized microstructure, and shear zones were formed inside of the grains.
MA
More shear zones formed inside of the grains and higher DRX fractions appeared in the AZ80 Mg alloy HECCAP-treated at a larger extrusion ratio or a larger conical mandrel angle, which led to a higher tensile yield strength, ultimate tensile strength, and
D
elongation. The highest ultimate tensile strength, tensile yield strength and elongation
TE
were 335 MPa, 308 MPa, and 7.2 %, respectively, when the extrusion ratio was 2.77 and the conical mandrel angle was 120°.
CE P
A formula was proposed to calculate the total generated plastic strain for HECCAP, which was found to increase with both the extrusion ratio and conical mandrel angle. Acknowledges
AC
This work was supported by the Major National Science and Technology Projects, No. ZX201204010101; the Fundamental Research Funds for the Central Universities,No. 30920140112008; Jiangsu Qinglan Project; Jiangsu National Natural Science Foundation, No. BK20151489. References [1] Zhu R, Wu YJ, Ji WQ, Wang JT. Cyclic softening of ultrafine-grained AZ31 magnesium alloy processed by equal-channel angular pressing. Mater Lett 2011; 65: 3593-6. [2] Zhang XP, Feng SF, Hong XT, Liu JQ. Orientation-related specimen thickness effects on mechanical properties of hot extruded AZ31B magnesium alloy. Mater Des 2013; 46:256-63. [3] Yakubtsov IA, Diak BJ, Sager CA, Bhattacharya B, MacDonald WD, Niewczas M. Effects of heat treatment on microstructure and tensile deformation of Mg AZ80 alloy 8
ACCEPTED MANUSCRIPT at room temperature. Mater Sci Eng A 2008; 496:247-55. [4] Zhao DG, Wang ZQ, Zuo M, Geng HR, Effects of heat treatment on microstructure and mechanical properties of extruded AZ80 magnesium alloy. Mater Des 2014;
T
56:589-93
IP
[5] Zhu R, Ji WQ, Wu YJ, Cai XT, Yu Y. Effect of aging treatment on low-cycle fatigue behavior of extruded Mg-8Al-0.5Zn alloys. Mater Des 2012; 41:203-7.
SC R
[6] Lv CL, Liu TM, Liu DJ, Jiang S, Zeng W. Effect of heat treatment on tension-compression yield asymmetry of AZ80 magnesium alloy. Mater Des 2012; 33: 529-33.
NU
[7] Zhang XP, Castagne S, Luo XF, Gu CF. Effects of extrusion ratio on the ratcheting behavior of extruded AZ31B magnesium alloy under asymmetrical uniaxial cyclic
MA
loading. Mater Sci Eng A 2011; 528:838-45.
[8] Chen F, Chen S, Dong XH, Li CY, Hong XT, Zhang XP. Size effects on tensile strength of aluminum-bronze alloy at room temperature. Mater Des 2015; 85:778-84.
D
[9]Ebrahimi R, Reihanian M, Moshksar MM. An analytical approach for
TE
radial-forward extrusion process. Mater Des 2012; 29: 1694-700. [10]Lee YS, Hwang SK, Chang YS, Hwang BB. The forming characteristics of
CE P
radial-forward extrusion. J Mater Process Technol 2001; 113:136-40 [11] Mogucheva A, Babich E, Ovsyannikov B,Kaibyshev R. Microstructural evolution in a 5024 aluminum alloy processed by ECAP with and without back pressure. Mater Sci Eng A 2013; 560:178–192
AC
[12] Kocich R, Macháčková A, Andreyachshenko VA. A study of plastic deformation behaviour of Ti alloy during equal channel angular pressing with partial back pressure. Comp Mater Sci 2015; 101: 233–241 [13] Ma SJ, Liu Y, Dong XH, Zhang XP. Microstructure and flow stress of Mg-12Gd-3Y-0.5 Zr magnesium alloy. J Wuhan Univ Technol-Mater Sci Ed 2013; 28 (1):172-7 [14] She J, Pan FS, Guo W, Tang AT, Gao ZY, Luo SQ, Song K, Yu ZW, Rashad M. Effect of high Mn content on development of ultra-fine grain extruded magnesium alloy. Mater Des 2016; 90(15)7-12 [15] Padhy GK, Wu CS, Gao S, Shi L. Local microstructure evolution in Al 6061-T6 friction stir weld nugget enhanced by ultrasonic vibration. Mater Des 2016; 92(15)710-23 [16] Kamran J, Shamas Ud Din, Tariq NH, Ali F, Hasan BA. The beneficial effect of 9
ACCEPTED MANUSCRIPT AgIn addition on deformation behavior, microstructure and texture in Mg–Al–Zn alloy during single pass warm rolling. Mater Des 2015; 81(15)11-20 [17] Zhang J, Fang C, Yuan FQ, Liu CP. A comparative analysis of constitutive
T
behaviors of Mg–Mn alloys with different heat-treatment parameters. Mater Des 2011;
IP
32(4)1783-9
[18] Hong XT, Chen F, Chen F, Yu W, Sang BR, Zhang XP. Effects of specimen
alloy. Adv Mater Res 2014; 1004-1005:158-62.
SC R
diameter on microstructure and microhardness of hot extruded AZ31B magnesium
[19] Sepahi-Boroujeni S, Fereshteh-Saniee F. The influences of the expansion equal
alloy. Mater Sci Eng A 2015; 636: 249-53
NU
channel angular extrusion operation on the strength and ductility of AZ80 magnesium
MA
[20]Chen Q, Zhao ZD, Zhao ZX, Hu CK, Shu DY. Microstructure development and thixoextrusion of magnesium alloy prepared by repetitive upsetting-extrusion. J Alloy Compd 2011; 509: 7303-15
D
[21] Cao Z, Wang FH, Wan Q, Zhang ZY, Jin L, Dong J. Microstructure and mechanical
2015; 67:64-71
TE
properties of AZ80 magnesium alloy tube fabricated by hot flow forming. Mater Des
CE P
[22] Park SH, You BS, Mishra RK, Sachdev AK. Effects of extrusion parameters on the microstructure and mechanical properties of Mg-Zn-(Mn)-Ce/Gd alloys. Mater Sci Eng A 2014; 598: 396-06.
[23] Barnett MR. Twinning and the ductility of magnesium alloys Part II: ''Contraction''
AC
twins. Mater Sci Eng A 2007; 464:8-16. [24] Park SH, Jung JG, Kim YM, You BS. A new high-strength extruded Mg-8Al-4Sn-2Zn alloy. Mater Lett 2015; 139:35-8. [25] Faraji G, Mashhadi MM, Kim HS. Tubular channel angular pressing (TCAP) as a novel severe plastic deformation method for cylindrical tubes. Mater Lett 2011; 65: 3009-12.
10
ACCEPTED MANUSCRIPT Figures captions Fig. 1 Schematic illustration of hydrostatic extrusion integrated with circular equal channel angular pressing process
T
Fig. 2 Placements of tensile specimen and microstructure specimen
IP
Fig. 3 Magnesium tube prepared by hydrostatic extrusion process integrated with circular equal channel angular pressing. (a) Whole tube, and (b) longitudinal section
SC R
Fig. 4 Microstructures and XRD result of AZ80 Mg alloy homogenized at 415 °C for 32h. (a)optical microscope, (b) and (c) SEM, and (d) XRD patterns Fig. 5 Typical microstrcutures of HECCAP-treated AZ80 Mg alloy. (a)OM of N side, (b)
NU
OM of S side, (c) SEM of S side, and (D) SEM of DRXed regions Fig. 6 Effects of ER on the microstructure. (a) 1.25, (b) 1.92, and (c) 2.77. CMA was
MA
120°
Fig. 7 Effects of ER on tensile properties of HECCAP-treated AZ80 Mg alloy Fig. 8 Microstructure of AZ80 Mg alloy HECCAP-treated with an ER of 1.25 and a
D
CMA of 105°
AC
CE P
TE
Fig. 9 Effects of CMA on tensile properties of HECCAP-treated AZ80 Mg alloy
11
CE P
TE
D
MA
NU
SC R
IP
T
ACCEPTED MANUSCRIPT
AC
Fig. 1 Schematic illustration of hydrostatic extrusion integrated with circular equal channel angular pressing process
12
MA
NU
SC R
IP
T
ACCEPTED MANUSCRIPT
AC
CE P
TE
D
Fig. 2 Placements of tensile specimen and microstructure specimen
13
AC
CE P
TE
D
MA
NU
SC R
IP
T
ACCEPTED MANUSCRIPT
Fig. 3 Magnesium tube prepared by hydrostatic extrusion process integrated with circular equal channel angular pressing. (a) Whole tube, and (b) longitudinal section
14
AC
CE P
TE
D
MA
NU
SC R
IP
T
ACCEPTED MANUSCRIPT
15
TE
D
MA
NU
SC R
IP
T
ACCEPTED MANUSCRIPT
CE P
(d)
1600
Mg
1200
Mg17Al12
AC
1400
Intensity
1000
800 600
400 200
0 20
30
40
50
60
70
80
90
2,
Fig. 4 Microstructures and XRD result of AZ80 Mg alloy homogenized at 415 °C for 32h. (a)optical microscope, (b) and (c) SEM, and (d) XRD patterns 16
AC
CE P
TE
D
MA
NU
SC R
IP
T
ACCEPTED MANUSCRIPT
17
AC
CE P
TE
D
MA
NU
SC R
IP
T
ACCEPTED MANUSCRIPT
18
D
MA
NU
SC R
IP
T
ACCEPTED MANUSCRIPT
TE
Fig. 5 Typical microstrcutures of HECCAP-treated AZ80 Mg alloy. (a)OM of N side,
AC
CE P
(b) OM of S side, (c) SEM of S side, and (D) SEM of DRXed regions
19
AC
CE P
TE
D
MA
NU
SC R
IP
T
ACCEPTED MANUSCRIPT
20
TE
D
MA
NU
SC R
IP
T
ACCEPTED MANUSCRIPT
AC
120°
CE P
Fig. 6 Effects of ER on the microstructure. (a) 1.25, (b) 1.92, and (c) 2.77. CMA was
21
ACCEPTED MANUSCRIPT
HECCAP-treated AZ80 Mg alloy tube at 220 C 340 CMA : 120 Ultimate tensile strength
IP
Elongation percentage
310 300 290 280
1.4
1.6
1.8
2.0
MA
260 1.2
NU
Tensile yield strength 270
SC R
Strength, MPa
320
T
330
2.2
2.4
10
8
6
4
2.6
Elongation percentage, %
350
2 2.8
Extrusion ratio
AC
CE P
TE
D
Fig. 7 Effects of ER on tensile properties of HECCAP-treated AZ80 Mg alloy
22
TE
D
MA
NU
SC R
IP
T
ACCEPTED MANUSCRIPT
AC
CMA of 105°
CE P
Fig. 8 Microstructure of AZ80 Mg alloy HECCAP-treated with an ER of 1.25 and a
23
ACCEPTED MANUSCRIPT
T
IP
340
SC R
320
300
280
260
MA
240 105
110
115
12 10 8 6 4
NU
Strength, MPa
14
HECCAPed AZ80 Mg alloy tube at 220 C ER was 2.77, tensile yield strength ER was 2.77,ultimate tensile strength ER was 1.92, tensile yield strength ER was 1.92,ultimate tensile strength ER was 2.77, elongation percentage ER was 1.92, elongation percentage
2
Elongation percentage, %
360
0 120
D
CMA,
AC
CE P
TE
Fig. 9 Effects of CMA on tensile properties of HECCAP-treated AZ80 Mg alloy
24
ACCEPTED MANUSCRIPT Table caption
AC
CE P
TE
D
MA
NU
SC R
IP
T
Table 1 EDS results of the locations shown in Figs. 4 (b)- (c)
25
AC
CE P
TE
D
MA
NU
IP
SC R
Table 1 EDS results of the locations shown in Figs. 4 (b)- (c) Location Mg, wt. % Al, wt. % A 92.14 7.86 B 93.20 6.80 C 79.61 20.39
T
ACCEPTED MANUSCRIPT
26
ACCEPTED MANUSCRIPT
AC
CE P
TE
D
MA
NU
SC R
IP
T
Graphical abstract
27
ACCEPTED MANUSCRIPT Highlights [1] Hydrostatic extrusion integrated with circular ECAP was proposed.
IP
T
[2] High properties AZ80 Mg alloy tube was prepared by HECCAP.
SC R
[3] Small diameter billet could be extruded into tube of larger diameter using the method.
[4]UTS, TYS and EP of the tubes were 335 MPa, 308 MPa, and 7.2 %, respectively.
NU
[5]A formula was proposed to calculate the total generated plastic strain for
AC
CE P
TE
D
MA
HECCAP.
28