Journal Pre-proof Experimental and numerical studies on the bending collapse of multi-cell Aluminum/ CFRP hybrid tubes Zhixin Huang, Xiong Zhang, Chongyi Yang PII:
S1359-8368(19)32544-2
DOI:
https://doi.org/10.1016/j.compositesb.2019.107527
Reference:
JCOMB 107527
To appear in:
Composites Part B
Received Date: 3 June 2019 Revised Date:
16 September 2019
Accepted Date: 10 October 2019
Please cite this article as: Huang Z, Zhang X, Yang C, Experimental and numerical studies on the bending collapse of multi-cell Aluminum/CFRP hybrid tubes, Composites Part B (2019), doi: https:// doi.org/10.1016/j.compositesb.2019.107527. This is a PDF file of an article that has undergone enhancements after acceptance, such as the addition of a cover page and metadata, and formatting for readability, but it is not yet the definitive version of record. This version will undergo additional copyediting, typesetting and review before it is published in its final form, but we are providing this version to give early visibility of the article. Please note that, during the production process, errors may be discovered which could affect the content, and all legal disclaimers that apply to the journal pertain. © 2019 Published by Elsevier Ltd.
1
Experimental and numerical studies on the bending collapse of
2
multi-cell Aluminum/CFRP hybrid tubes
3
Zhixin Huanga, Xiong Zhanga,b ∗ Chongyi Yanga
4
a Department of Mechanics, Huazhong University of Science and Technology, Wuhan 430074, Hubei, PR China
5
b Hubei Key Laboratory of Engineering Structural Analysis and Safety Assessment, Luoyu Road 1037, Wuhan 430074, PR China
6
Abstract: Wrapping the structures with composites and adopting multi-cell sections are two typical methods to
7
improve the crashworthiness of thin-walled beams. However, the effects of combining these two methods on
8
crashworthiness are not clear. This paper aims to investigate the bending collapse and crashworthiness of the multi-cell
9
aluminum/carbon fiber reinforced plastic (Al/CFRP) hybrid tubes under quasi-static and dynamic loading. Three-point
10
bending tests are firstly conducted for the CFRP, Al and Al/CFRP square tubes with single or multi-cell sections. The
11
deformation characteristics and crushing force responses of the tubes are analyzed, and the energy absorption
12
performances are evaluated. The bending resistance of the Al tubes is increased by up to 41% attributed to the CFRP
13
enhancement. The non-linear finite element software ABAQUS/Explicit is then employed to simulate the tests and help
14
analyze the deformation mechanisms. Parametric studies are performed to investigate the influence of the Al wall
15
thickness, the number of CFRP plies, loading velocity, partial wrapping and sectional shape on the crashworthiness of
16
Al/CFRP tubes. Results show that the Al wall thicknesses, partial wrapping, and sectional shapes have a significant
17
influence on the deformation pattern and force response of Al/CFRP tubes, while the number of CFRP plies and the
18
loading velocity have a relatively small influence. The specific energy absorption of Al/CFRP tubes can be increased
19
by 11% by introducing partial CFRP wrapping, and in all cases, the multi-cell Al/CFRP tubes outperform the single-
20
cell counterparts in crashworthiness performances.
21
Key words: Bending collapse; Al/CRFP hybrid tubes; Multi-cell section; Impact loading; Crashworthiness.
22 23
1. Introduction
24
In the vehicle industry, thin-walled beams are widely used as energy absorption components to
25
protect the occupants from injury [1-2]. The energy absorption performances of the beams under
26
various loads have attracted great interests in the scientific community [3-15], and continuous efforts
∗
Corresponding author. Tel.: +86 2787543538; fax: +86 2787543501.
E-mail address:
[email protected] (X. Zhang).
1
27
are made by researchers to explore the collapse mechanisms and improve the crashworthiness of the
28
thin-walled beams.
29
Bending collapse is an important energy dissipation mechanism of thin-walled beams under
30
lateral loads. A large number of studies were carried out on the bending collapse of thin-walled beams
31
by researchers. In 1983, Kecman [16] firstly proposed a theoretical model to predict the pure bending
32
response of thin-walled rectangular section tubes. Then, the pure bending collapse mechanisms were
33
further studied by Wierzbicki et al. [17] and Kim and Reid [18], and closed-form solutions were
34
derived for the moment-rotation response. Considering that pure bending is seldom encountered in
35
real crash events, recently researchers exerted more efforts on the three-point bending collapse of thin-
36
walled beams with various sectional shapes. The three-point bending collapse of thin-walled
37
rectangular tubes was recently studied by Huang and Zhang [19-20]. Two typical deformation modes:
38
bending collapse and bending with indentation were identified by them, and theoretical methods were
39
proposed to predict the moment or force responses. The collapse of dual rectangle tubes under three-
40
point bending was addressed by Bai et al. [21], and an analytical solution is also derived for the
41
bending response. The collapse resistance of various multi-cell tubes under three-point bending was
42
analyzed by Wang et al. [22], and the specific energy absorption (SEA) of the multi-cell sections was
43
reported to be over 50% higher than that of the single-cell counterparts. However, all these studies
44
only deal with the bending collapse of metallic beams.
45
In recent years, composite structures have been increasingly applied to the vehicles to improve
46
the fuel economy [23-24]. The composites have the advantages of high strength and lightweight, but
47
the brittle fracture of composites may significantly impair the crashworthiness of the structures. This
48
phenomenon was widely observed in the bending processes of composite structures. For example,
49
Gliszczyński et al. [25] investigated the pure bending of glass fiber reinforced plastic (GFRP) channel
50
section profiles, and the failure of fibers led to a significant decrease of the bending moment. The
51
three-point bending of square and double hat-shaped carbon fiber reinforced plastic (CFRP) beams
52
was studied by Liu et al. [26-27], and the fiber breakage resulted in sharp drops of the force responses
53
and low energy absorption efficiency.
2
54
The metal/composite hybrid beams have been recently adopted as an effective approach to
55
achieve lighter weight and better crashworthiness [28-29]. The metal/composite hybrid beams
56
combine the merits of both the metal and composite. The good plasticity of metal and high specific
57
strength of the composite can bring a strong hybrid structure. In recent years, the crashworthiness of
58
the hybrid structures under transverse loads has been addressed by many researchers. Shin et al. [30]
59
studied the three-point bending collapse of Al/CFRP hybrid square tubes, and the bending resistance
60
was greatly affected by the lay-up sequence of the laminates. The bending response of Al/GFRP tubes
61
was investigated by Jung et al. [31], and the SEA of the hybrid tube was found 29% higher than that
62
of the Al counterpart. The collapse characteristics of Al/CFRP circular beams under three-point
63
bending were analyzed by Sun et al. [32], and the SEA value of the hybrid structure was increased by
64
43% by structural optimization.
65
It is noted that most of the current studies are concerned with the collapse of metallic profiles,
66
pure composite structures, and single-cell metal/composite beams. Up to now, there are still no studies
67
on the bending collapse of metal/composite beams with multi-cell sections. Since the metallic multi-
68
cell sections exhibit high bending resistance and good energy absorption performances [21-22, 33],
69
the crashworthiness and collapse mechanisms of multi-cell metal/composite hybrid tubes under three-
70
point bending will be quite noteworthy and interesting.
71
This paper aims to study the bending collapse of multi-cell Al/CFRP hybrid tubes. Quasi-static
72
and dynamic three-point bending tests are first conducted for the pure CFRP, Al and Al/CFRP square
73
tubes with single or multi-cell sections. The nonlinear finite element software ABAQUS/Explicit is
74
then employed to simulate the tests and help analyze the collapse mechanisms. Finally, parametric
75
studies are carried out to investigate the influences of the Al wall thickness, the number of composite
76
layers, loading velocity, partial CFRP wrapping, and sectional shape on the bending responses and
77
crashworthiness of Al/CFRP hybrid tubes.
78
2. Specimens and experimental setup
79
2.1 Specimens preparation
3
80
Aluminum multi-cell square profiles and WP-3011 plain woven carbon fiber/epoxy prepreg are
81
employed to fabricate the Al, CFRP, and Al/CFRP hybrid specimens. The representative Al specimens
82
are shown in Fig. 1(a), and two different sectional shapes: double-cell and quadruple-cell sections are
83
adopted. The length of the Al tubes is 270 mm, and the outside sectional dimension is 32 mm × 32
84
mm. The wall thicknesses of the outside and inside plates of the multi-cell sections are slightly
85
different. As indicated in Fig. 1(b), the thicknesses of the outside plates and inside ribs are 0.95 and
86
1.01 mm, respectively.
87
In the fabrication of pure CFRP specimens, three layers of the prepregs are wrapped on the Al
88
tubes with a layer of demolding film between them, and they are then enclosed and cured in a furnace.
89
The curing temperature is controlled as follows: the temperature is linearly increased to 120 ℃ in 90
90
minutes, and then kept constant for 90 minutes, and finally cooled down to the room temperature.
91
After the curing process, the pure CFRP specimens can be taken out from the Al tubes by demolding.
92
Due to the manual operation errors and spring back of the composite, small fillets are developed for
93
the CFRP sections, and the fillet radius is measured to be 2 mm.
94
During the fabrication of Al/CFRP hybrid specimens, the Al tubes are first treated by using a
95
phosphoric acid anodizing method to achieve good adhesion with CFRP layers. The outside tube
96
surfaces are then wrapped with three layers of prepregs, and finally, the hybrid beams are cured with
97
the same process as the pure CFRP specimens.
98
The representative CFRP and Al/CFRP tubes are also shown in Fig. 1(a). For the sake of
99
convenience, the pure CFRP, double-cell and quadruple-cell Al specimens are denoted by CFRP, A2,
100
and A4, respectively. The Al/CFRP hybrid tubes with double-cell and quadruple-cell sections are
101
distinguished by CA2 and CA4, respectively.
102
2.2 Material properties
103
The material of the Al tubes is AA6063-O. According to ASTM E8M-04 [34], the constitutive
104
relation of the material is obtained by performing uniaxial tensile tests on a 10 KN capacity Zwick
105
Z010 universal test machine. The engineering stress-strain curves of AA6063-O are plotted in Fig. 2
4
106
(a). The mechanical properties are as follows: density ρ = 2.7 g/cm3, Young's modulus E = 68.9 GPa,
107
Poisson's ratio ν = 0.33, the initial yield stress σy = 30.1 MPa and the ultimate stress σu = 106.1 MPa.
108
The WP-3011 plain woven carbon fiber/epoxy prepregs are manufactured by Weihai Guangwei
109
Composite Company. The weight per square meters of the prepreg is 330 g/m2, and the resin content
110
is 40%. The thickness of the carbon fiber woven fabric is 0.25 mm. In order to obtain the mechanical
111
properties of composites, several experimental tests are conducted according to related test standards,
112
including the tensile (ASTM D3039 [35]), compression (ASTM D695-10 [36]) and in-plane shear
113
(ASTM D3518 [37]) tests. The stress-strain curves of CFRP under tensile, compression and in-plane
114
shear tests are plotted in Fig 2. (b) - (d). Since the interfacial properties are critical for collapse
115
responses, the bonding strengths between CFRP and CFRP or CFRP and Al in normal and shear
116
directions are also tested, and the curves for bonding strength are given in Fig 2. (e) - (h).
117
The damage initialization and evolution of composites are associated with the critical fracture
118
energy. The related fracture energy for the same type of composite WP-3011 produced by the same
119
company was tested by Sun et al. [14], although the strengths of the present material are slightly
120
different. The fracture energy data measured by them are employed here. According to Sokolinsky et
121
al. [38], the critical fracture energy is approximately linearly correlated to the strength [38]. The
122
critical fracture energies for composite failure and interfacial damage are hence linearly adjusted
123
accordingly. The detailed values of the CFRP mechanical properties are presented in Section 5 for the
124
numerical study.
125
2.3 Experimental setup
126
Figure 3 illustrates the schematic diagram and experimental setups for the quasi-static and
127
dynamic impact three-point bending tests. In the two loading cases, the radius of the cylindrical punch
128
and supports is R=12 mm, and the span between the two supports is S=180 mm. Two repetitions are
129
tested in each case.
130
The quasi-static bending tests are performed on a 100 kN capacity universal testing machine with
131
computer control and data acquisition system. The loading speed is kept constant to be 1 mm/s, and
5
132
the stoke distance is set as δ=85 mm. For the pure CFRP tubes, the loading process is manually
133
terminated, when the reaction force drops to almost zero.
134
The dynamic impact tests are conducted on a drop-hammer test machine. The total mass of the
135
hammer is 78.1 kg, and the release height is set as 1.35 m above the specimens. Due to the influence
136
of friction, the impact velocity is measured to be 5.1 m/s before the hammer contacts with the
137
specimens. The stroke distance in the impact tests is δ=87.5 mm, and two buffers are put below the
138
hammer to terminate the impact process.
139
3. Quasi-static tests
140
3.1 Deformation process and force response
141
In the quasi-static tests, the deformation processes of the specimens are recorded by a video
142
camera. In all cases, the two repetitions of the specimens show almost the same deformation behavior.
143
Figure 4 presents a typical deformation process of the pure CFRP tubes. When the punch is in contact
144
with the CFRP, inter/intra-lamina cracks are first generated for the composites in the upper corners.
145
With the ongoing of the loading, the cracks on the top flange propagate from the corners to the center,
146
while those on the web plates spread from top to bottom. Finally, the fibers in the top flange and web
147
plates are completely fractured, and asymmetric deformation is observed for the structures.
148
The force-displacement curves of the pure CFRP tubes are shown in Fig. 5(a). The response
149
curves can be generally divided into two stages. In the first stage, the crushing force increases to a
150
peak rapidly, and it then drops gradually in the second stage. It is obvious that the pure CFRP tubes
151
are not desirable for energy absorption since the fiber break significantly reduces the load bearing
152
capability and load uniformity of the structure.
153
The deformation processes of A2 and A4 in the quasi-static tests are presented in Fig. 6. The two
154
Al multi-cell sections show similar deformation behavior. The plastic deformation is first formed in
155
the areas beneath the punch, and it then expands to the adjacent regions. The punch indents into the
156
tube and almost the whole cylindrical punch head is enclosed by the deformed flange and web plates.
157
The force-displacement curves of the Al tubes are plotted in Fig 5(b) and (c). The two Al sections
158
show different force response tendencies since the bending resistance of thin-walled beams is
6
159
significantly affected by the sectional shape. For A2, the crushing force increases rapidly to an initial
160
peak and then decreases to some extent. After that, the force rises again to a much higher second peak
161
and finally drops again. As for A4, the crushing force increases fast to an initial peak and then keeps
162
rising to a second peak, and finally declines gradually.
163
Figure 7 presents the deformation behavior of CA2 and CA4. The collapse of these hybrid tubes
164
is dominated by the plastic deformation of the Al multi-cell profiles and accompanied by the failure of
165
the CFRP. The significant local indentation and global bending co-occur for the tubes in the
166
deformation processes, and the CFRP in the center region is completely broken. Generally, the CFRP
167
restrains the outward deformation of the Al walls, while the deformation of the Al walls and the
168
compression of the punch lead to the failure of the CFRP.
169
The force response curves of CA2 and CA4 are plotted in Fig. 5(d) and (e), respectively. It is
170
noted that the crushing force drops sharply at the approximate δ=45 mm due to the tensile fracture of
171
fibers in the bottom flange in the center region. The force response curves can be divided into two
172
stages by taking δ=45 mm as the boundary. In the earlier stage, the crushing force of the CA2 rises to
173
the initial peak and then descends, and finally, it increases again, while that of the CA4 keeps
174
increasing slowly after the initial peak. In the later stage, after the drastic drop, the force of the CA2
175
keeps almost constant, while that of the CA4 increases gradually. Figure 5(f) compares the force
176
responses of various specimens. Due to the CFRP enhancement, the Al/CFRP tubes get much higher
177
crushing force than their Al counterparts.
178
The final deformed shapes of the specimens in the quasi-static tests are presented in Fig. 8. For
179
the pure CFRP tubes, the cracks are concentrated on the top flange and web plates, while the bottom
180
flange is almost undamaged. The center part of one CFRP specimen breaks into fragments, and the
181
fragments are not shown here. Furthermore, the CFRP tubes almost revert to the initial straight state
182
after unloading due to the spring back of the material.
183
As for the Al tubes, the top flange collapses inward, and multi-folds are formed on the top flange
184
and web plates. The global bending is accompanied by the local indentation for these tubes. This
185
deformation mode is attributed to the relatively lower indentation resistance and higher bending
7
186
resistance of the beams, as addressed by Huang and Zhang [19-20]. The deformed shapes of the
187
Al/CFRP tubes are similar to those of the Al tubes. The inner Al parts are bent with significant local
188
indentation, and the CFRP around the punch is completely fractured.
189
3.2 Energy absorption characteristics
190
To better understand the influence of the composite wrapping on the energy absorption
191
performance of the tubes, the energy absorption indices are calculated in two different displacement
192
ranges. The first range is between 0 and 45 mm to exclude the complete fracture of composite, while
193
the other covers the whole loading process.
194
The energy absorption indices in these two ranges are summarized in Table 1. The indices
195
include the energy absorption E, mean crushing force Pm, and specific energy absorption SEA (energy
196
absorption per unit mass). Due to the brittle fracture of the composite, the Pm and SEA values of
197
CFRP tubes are much lower than those of the Al and Al/CFRP tubes. By introducing the CFRP
198
wrapping, the Pm values of A2 and A4 are increased by 27% and 41% in the first stage. Considering
199
the mass increase due to CFRP wrapping, the SEA of A2 in the first range is decreased by 3%, while
200
that of A4 is increased by 10%. In the whole range, the Pm values of CA2 and CA4 are 28% and 36%
201
higher than those of their Al counterparts, respectively. In this case, the CFRP wrapping still almost
202
has no improvement on the SEA of CA2, while the SEA of A4 is increased by 7%.
203
The energy absorption of the Al/CFRP tubes is also affected by the interaction between Al and
204
CFRP parts, just as addressed by Sun et al. [32]. To investigate the interaction effect, we compare the
205
energy absorption E of the hybrid tubes with the sum of that of the corresponding Al and CFRP tubes.
206
The total energy absorption E is calculated within the first 40 mm in the distance, since the pure CFRP
207
tubes almost have no load carrying capacity when the crushing distance exceeds 40 mm. The sum of
208
the energy absorption of A2 and CFRP is 89.17 J, and that of A4 and CFRP is 111.94 J. As for the
209
hybrid tubes, the E values of CA2 and CA4 are 94.74 and 134.20 J, respectively. The relatively higher
210
E values of the hybrid tubes indicate that the contribution of the interaction effect on energy
211
absorption is 6.3% and 19.9% for the CA2 and CA4, respectively.
212
4. Dynamic impact tests 8
213
4.1 Deformation mode and force response
214
Figure 9 shows the deformed shapes of the double-cell and quadruple-cell Al and Al/CFRP tubes
215
in the dynamic impact tests. All the specimens exhibit global bending deformation with local
216
indentation features, and the CFRP layers of the hybrid tubes are broken into two segments in the
217
center areas. The deformed shapes of the specimens in quasi-static and dynamic tests are compared in
218
Fig. 10. Generally, the deformation modes in the dynamic tests are similar to those in the quasi-static
219
loading. However, obvious asymmetric deformation is observed for A2 and CA2 specimens in the
220
dynamic loading, whose web plates tilt to one side in the lateral direction. Theoretically, the
221
deformation of the middle rib breaks the balance of the stress distribution of the multi-cell sections
222
and leads to the asymmetric deformation of the structures. This asymmetric deformation is aggravated
223
in the dynamic loading and reduced to some extent by introducing the CFRP wrapping.
224
The force-displacement curves of the specimens in the dynamic tests are plotted in Fig. 11. In all
225
cases, the two repetitions give almost the same force responses, and the only small difference is
226
observed for the curves of A2 in the later stage. This difference should be attributed to the slight
227
difference in their asymmetric deformation processes. When compared with the quasi-static results,
228
the dynamic force responses show four different features. Firstly, the crushing force in the dynamic
229
loading fluctuates more violently than that in the quasi-static loading. Second, the initial peak force in
230
the impact tests is much higher. The inertia effect in the dynamic loading should be the major reason
231
for this. Third, the crushing force drops sharply at about δ=87.5 mm in the dynamic tests. This drop is
232
due to the action of the buffers, and the loading process is then terminated. Fourth, in dynamic loading,
233
the CFRP in the center area is wholly broken at δ=35 mm, which leads to the drastic drop of the
234
crushing force. However, the CFRP is broken at δ=45 mm in the quasi-static tests. It seems that the
235
CFRP is easier to fracture in the dynamic loading.
236
4.2 Energy absorption indices
237
In the dynamic loading, the energy absorption indices are also calculated in two different ranges,
238
which is the same as done in quasi-static loading. The crashworthiness indices are listed in Table 2.
239
Due to the CFRP enhancement, the mean crushing forces of A2 and A4 are increased by 12% and 24%
9
240
in the first stage, while the increase rates are 21% and 28% in the whole stage. Due to different
241
structural masses, the SEA values of CA2 are 16% and 9% lower than those of A2 in the first stage
242
and whole process, respectively. For A4 and CA4, the calculated Pm and SEA values are almost the
243
same in these two ranges.
244
The energy absorption indices in quasi-static and dynamic tests are compared here to investigate
245
the dynamic effect. For the first stage, the dynamic mean crushing forces of the Al tubes are 14%-16%
246
higher than the quasi-static results, while the Pm values in the two load cases are identical for the
247
Al/CFRP hybrid tubes. In the whole stage, compared with the quasi-static results, the dynamic Pm
248
values of A4 and CA4 are increased by 14% and 7%, respectively. However, the dynamic mean
249
crushing force of A2 is equal to the quasi-static one, while that of CA2 is even 5% lower than the
250
quasi-static result in the whole process. The non-increase of Pm is due to the aggravated asymmetric
251
deformation of the double-cell sections in dynamic loading (in Fig. 10), which decreases the structural
252
collapse resistance. The index SEA shows a similar tendency as Pm in the two loading conditions.
253
5. Numerical simulation
254
5.1 Finite element model
255
The quasi-static and dynamic experimental tests are simulated by utilizing the commercial finite
256
element software ABAQUS/Explicit. Figure 12(a) shows the finite element model for the impact test
257
of quadruple-cell Al/CFRP tubes, which is a representative model for all the tests. The numerical
258
model includes five parts: the punch, supports, the Al profile, CFRP plies, and the adhesive layers.
259
The rigid element (R3D4) was employed to model the punch and supports. The Al and CFRP parts are
260
discretized by conventional shell elements (S4R). The cohesive element (COH3D8) is used to model
261
the adhesive layers. A mesh sensitivity analysis is performed to determine the mesh size. Three
262
different mesh sizes: 0.5, 1.0, and 1.5 mm are adopted for the impact analysis of CA4, and the force-
263
displacement curves are shown in Fig. 12(b). It is noted that the mesh size of 1.0 mm is fine enough to
264
achieve good accuracy and is employed in the following analysis.
265
In the numerical model, the surface to surface contact is defined to simulate the interaction
266
between specimens and the punch or supports, and the general contact is applied to account for the
10
267
self-contact of the specimens. Considering the different surface roughness, for the pure Al tubes, the
268
friction coefficient for all the contacts is 0.3 [20], while for the pure CFRP and Al/CFRP tubes, it is
269
set as 0.1 [30].
270
For the quasi-static simulations, the loading speed has to be increased to complete the
271
calculations in a reasonable time. According to the principles proposed by Santosa et al. [39], the
272
loading speed is ramped to 1 m/s in the first 20 ms and then kept constant in the remaining process. In
273
the simulation the impact tests, a point mass of 78.1 kg is applied in the center of the punch. The
274
initial velocity of the punch is set as 5.1 m/s. The gravitational acceleration is defined as 9.81 m/s2 for
275
all the parts.
276
According to the ABAQUS documentation [40], the aluminum material is modeled by the elasto-
277
plastic constitutive model, and the true stress-strain data converted from the engineering stress-strain
278
curves are used as input. The traction separation law is defined for the cohesive elements.
279
The thickness of these elements is specified as 0.1 mm and the related parameters are given in Table 3.
280
The constitutive model of the CFRP plies is implemented by a user-defined material subroutine
281
VUMAT. Detailed information about the traction-separation law and the VUMAT subroutine has
282
been introduced in references [38, 41-42], and it is hence not presented here. The mechanical
283
properties of the CFRP are listed in Table 4, and the related parameters for the plastic and failure
284
behaviors of CFRP under shear loading are summarized in Table 5.
285
5.2 Numerical results
286
According to the experimental results, the deformation and failures of the specimens are mainly
287
concentrated in the areas around the punch. In this subsection, the simulated deformation
288
characteristics in the center region of the specimens are compared with the experimental results. For
289
the pure CFRP and Al/CFRP tubes, the tensile damage statuses along the warp direction (SVD1) of
290
the CFRP are given in the numerical results. As for the pure Al tubes, the Von Mises stress of the
291
structures is plotted in the simulation results.
292
The deformation processes of the pure CFRP, Al and Al/CFRP tubes in the quasi-static tests are
293
shown in Figs. 4, 6, and 7, respectively. It is noted that the deformation behaviors in simulations are in
11
294
good agreement with those in the experiments. Figure 8 presents the final deformed shapes of the
295
tubes in the quasi-static loading, and the simulations give almost the same deformation patterns as the
296
experiment for the Al and Al/CFRP tubes. For the pure CFRP tubes, the simulated deformed shape is
297
different from the experiment, since the spring back of CFRP after unloading is not considered in the
298
simulation. The deformed shapes of tubes in the dynamic loading are presented in Fig. 9. The
299
simulation and experiment results compare fairly well.
300
The force-displacement curves of the specimens in quasi-static and dynamic loading are plotted
301
in Fig. 5 and 11, respectively. The simulated crushing force responses show good agreement with the
302
experiment results. To further understand the differences between simulation and experimental results,
303
the mean crushing forces in simulation (Pm-simu) are compared with the average mean forces in
304
experiments (Pm-avg). As shown in Table 1 and 2, the error of the mean crushing force (Pm-simu/Pm-avg –
305
1) is 13.3% for the pure CFRP specimens, while it is less than 7.2% for the Al and Al/CFRP hybrid
306
tubes.
307
Considering the high diversity of CFRP failure behavior, the present finite element model
308
simulates the three-point bending response of the thin-walled tubes with an excellent accuracy. The
309
numerical model is hence employed to perform the parametric study on the bending collapse
310
responses of the Al/CFRP hybrid tubes.
311
6. Parametric study and discussion
312
In this section, parametric studies are performed to investigate the influences of several critical
313
factors on the bending responses of Al/CFRP tubes. These factors include the Al wall thickness, the
314
number of CFRP plies, loading velocity, partial CFRP wrapping, and sectional shape. In the
315
parametric analyses, the dimensions of the square Al profiles are kept unvaried as the length L=270
316
mm and outside width b=32 mm. The numerical model validated in the previous section is adopted,
317
and the default parameters in the simulations are set as the Al wall thickness t=1.0 mm, the number of
318
CFRP plies n=3 and initial velocity V=5.1 m/s. When the effect of one factor is investigated, other
319
parameters are kept constant. The stroke distance is set to δ=80 mm, and the crashworthiness indices
12
320
are also calculated in two different ranges: the first one covers the first half stage 0-40 mm, and the
321
second one includes the whole process 0-80 mm.
322
6.1 Al wall thicknesses
323
The wall thickness of the Al profiles is a critical factor for the bending responses of the hybrid
324
tubes. Numerical simulations are performed for double-cell and quadruple-cell Al/CFRP tubes with
325
three different Al wall thicknesses: t=1.0, 1.5 and 2.0 mm to analyze its influence.
326
The deformed shapes of the Al/CFRP tubes are shown in Fig. 13. It is noted that the CFRP plies
327
in the center areas are wholly fractured, and the hybrid tubes show two different deformation modes:
328
bending with indentation and bending collapse. The deformation mode of a tube is determined by the
329
relative strength on the resistance of the bending collapse and local indentation. Due to the relatively
330
lower indentation resistance of thin Al sections, CA2 and CA4 with t=1.0 mm deform in the bending
331
with indentation mode. For t=1.5 and 2.0 mm, the bending collapse mode is developed for the hybrid
332
tubes.
333
Figure 14 presents the force-displacement curves of the Al/CFRP tubes with three different Al
334
wall thicknesses. In general, the increase of t results in higher crushing force and smaller distance for
335
the sharp drop of the force. However, the sharp drop is not significantly observed for CA2 with t=1.0
336
mm, which is similar to that of CA2 in the dynamic impact tests (in Fig. 11). This occurrence may be
337
associated with the severe asymmetric deformation of the relatively thin double-cell section. This
338
severe asymmetric deformation leads to the torsion and skew of the beam and primarily results in the
339
shear failure of the fibers in the bottom flange, instead of the tension fracture.
340
The energy absorption indices of the Al/CFRP tubes are calculated in Table 6. When t increases
341
from 1 mm to 2 mm, the Pm of CA2 and CA4 are increased by 153% and 140% in the first stage, and
342
by 108% and 113% in the whole process, respectively. The increments of SEA for CA2 and CA4 are
343
up to 43% and 34% in the first stage, and 17% and 18% in the whole stage. It can be concluded that
344
the increase of Al wall thickness is an effective approach to increase the crashworthiness of the
345
Al/CFRP tubes.
346
6.2 The number of CFRP plies
13
347
The influence of the number of CFRP plies on the collapse responses of the Al/CFRP tubes is
348
investigated here. Numerical simulations are carried out for CA2 and CA4 tubes with 3, 5 and 7 layers
349
of CFRP.
350
The deformed shapes of the Al/CFRP tubes are presented in Fig. 15. All these tubes develop the
351
bending with indentation mode, and the CFRP layers in the central region are completely broken. The
352
force-displacement curves of the tubes are plotted in Fig. 16. It is noted that the crushing force is
353
increased with the increase in the number of CFRP plies.
354
The energy absorption indices of the Al/CFRP tubes are listed in Table 7. Due to the
355
enhancement of CFRP, the Pm of CA2 and CA4 is increased by 23%-47% and 20%-35% in the first
356
stage, and 18%-40% and 16%-31% in the whole process. Considering the increase in structural mass,
357
the increase of CFRP layers has a slight improvement on the SEA of CA2 (6%-12%) and CA4 (5%-
358
6%) in the first stage, while it almost has no enhancement on SEA in the whole process.
359
6.3 Loading velocity
360
The influence of loading velocity on the crashworthiness of the Al/CFRP tubes is investigated in
361
this subsection. Numerical simulations are performed for Al/CFRP tubes loaded with three different
362
initial velocities V=5.1, 15 and 25 m/s.
363
The deformation patterns of the tubes are shown in Fig. 17. All these tubes deform in the bending
364
with indentation mode, and the CFRP in the center is completely fractured. The force response curves
365
of the tubes are plotted in Fig. 18. The increase of the initial loading velocity leads to much higher
366
force levels in the initial stage (δ < 10 mm), while it has a small influence on the crushing force in the
367
subsequent stages.
368
The energy absorption indices of the Al/CFRP tubes are summarized in Table 8. It is noted that
369
both Pm and SEA values are increased with the increase of the loading velocity. When the initial
370
loading velocity is increased from 5.1 m/s to 25 m/s, the Pm values of CA2 and CA4 are increased by
371
22% and 25% in the first stage, and 19% and 20% in the whole process, respectively. The SEA shows
372
a similar tendency as Pm when the loading velocity is varied.
373
6.4 Partial wrapping of CFRP
14
374
According to the previous analyses, the deformation is localized around the punch, and the CFRP
375
far from the center region is almost undamaged. To achieve higher energy absorption efficiency,
376
partial wrapping of CFRP on the Al tubes should be a quite promising method, since it can improve
377
the bending resistance of the beams with less mass. The effect of partial CFRP wrapping on the
378
crashworthiness of the Al/CFRP tubes is analyzed here. For simplicity, a parameter λ is defined as the
379
ratio of the length of the CFRP reinforced region to the whole tube length. Al/CFRP tubes with four
380
different λ=1.0, 0.75, 0.50 and 0.25 are analyzed.
381
Figure 19 shows the deformed shapes of the Al/CFRP tubes with partial CFRP wrapping. With
382
the decrease of λ, the deformation mode of CA2 switches from bending with indentation to bending
383
collapse. Nevertheless, the variation of λ almost does not affect the deformation mode of CA4, which
384
is bending with significant local indentation. For CA4 with λ=0.25, the CFRP wrapping region is
385
smaller than the plastic deformation area of Al tube, and the whole CFRP is debonded from the Al
386
profile.
387
Figure 20 plots the force-displacement curves of the tubes with partial CFRP wrapping. It is
388
noted that the force response curves for different λ values at λ>0.25 are almost overlapped for both
389
CA2 and CA4, while the reaction force level is much lower at λ=0.25. The lower crushing force of
390
CA2 at λ=0.25 is due to the switch of the deformation mode [19], while that of CA4 is attributed to the
391
debonding between the Al and CFRP.
392
The energy absorption indices of the Al/CFRP tubes are given in Table 9. For both CA2 and CA4,
393
the Pm values of λ=1.0, 0.75 and 0.5 show very slight difference in the collapse processes, while those
394
of λ=0.25 are much lower. With the decrease of λ, the SEA of CA2 is increased by 6%-11% in the first
395
stage. As for the entire process, the SEA of CA2 is increased by 5-8% at λ=0.75 and 0.50, while it
396
decreased by 16% at λ=0.25 due to the mode switch. When λ decreases from 1 to 0.25, the SEA of
397
CA4 is increased by up to 11% in both the first stage and whole process.
398
6.5 Sectional shapes
399
The sectional shape is a crucial factor for the crashworthiness of Al/CFRP tubes. To investigate
400
its influence, Al/CFRP tubes with single (CA1), double (CA2), quadruple (CA4) and nonuple (CA9)
15
401
cells are analyzed here. Two different cases are discussed: tubes with constant Al wall thickness (t=1.0
402
mm) and those with constant mass (m=170.85 g).
403
The deformation modes of the Al/CFRP tubes are plotted in Fig. 21. In the case of constant
404
thickness, all the tubes deform in the bending with indentation mode, while for the constant mass case,
405
CA1 and CA2 deform in the bending collapse mode, and CA4 and CA9 develop the bending with
406
indentation mode. In the later case, there is a shift of the deformation mode from bending collapse to
407
bending with indentation. This is reasonable since the wall thickness is decreased with the increase of
408
sectional cell number when the mass is kept unvaried, and thinner tubes are more ready to trigger local
409
indentation.
410
Figure 22 presents the force response curves of the tubes. In the case of constant thickness, the
411
increase of the sectional cell number results in a much higher crushing force, and the sharp drop in
412
crushing force is observed for CA4 and CA9. In the case of constant mass, the crushing force before
413
the sharp drop shows a comparable level for all sections. However, CA1 shows considerably lower
414
force level than other sections in the later stage. This is due to the fact that the resistance for bending
415
collapse mode is relatively low, and multi-cell sections achieve higher crushing force than the single-
416
cell counterpart at a relatively large loading distance [22].
417
Table 10 lists the energy absorption indices of the tubes. In the case of constant thickness, the Pm
418
and SEA are increasing with the increase in the number of sectional cells. When the cell number
419
increases from 1 to 9, the Pm values are increased by 125% and 127% in the first stage and the whole
420
process, respectively. At the same time, the SEA is increased by 31% and 32%, respectively. In the
421
case of constant mass, the energy absorption capacity and efficiency of the tubes are growing with the
422
increase of the number of sectional cells. Among these sections, CA9 achieve the highest Pm value,
423
which is 10% and 44% higher than that of CA1 in the first stage and the whole process. Due to the
424
constant mass, the influence of sectional shapes on SEA is the same as that on Pm.
425
7. Conclusion
426
The quasi-static and dynamic three-point bending collapse of multi-cell Al/CFRP square tubes is
427
studied in this paper. The quasi-static and dynamic three-point bending tests are performed for the
16
428
CFRP, Al and Al/CFRP tubes with single, double-cell or quadruple-cell sections first. The deformation
429
characteristics and force responses are then analyzed. The non-linear finite element software
430
ABAQUS/Explicit is employed to simulate the tests and perform the parametric studies. The
431
influences of several critical factors on the bending responses of Al/CFRP tubes are discussed. The
432
major conclusions are summarized as follows:
433
(1) In the quasi-static and dynamic bending tests, all the Al and Al/CFRP specimens collapse in the
434
bending with indentation mode, and the complete fracture of composite in the center region leads
435
to sharp drops in the crushing force of Al/CFRP tubes.
436
(2) The pure CFRP tubes are not efficient for energy absorption due to the brittle fracture during the
437
loading. By introducing the CFRP wrapping, the Pm of the Al tubes is increased by 12%-41%,
438
while the SEA of the tubes is decreased or slightly improved due to the mass increase.
439
(3) The deformation mode and force responses of the tubes in the simulations compare well with the
440
experimental results. The error of Pm is 13.3% for the pure CFRP specimens, while it is less than
441
7.2% for the Al and Al/CFRP hybrid tubes.
442
(4) The deformation mode of the Al/CFRP tubes is determined by the relative strength on the
443
resistance of bending collapse and local indentation. The Al wall thickness, partial CFRP
444
wrapping, and sectional shape have a significant influence on the deformation mode, while the
445
number of CFRP plies and the initial loading velocity of the punch only have a small influence.
446
(5) The increase of the Al thickness can increase both the Pm and SEA of the Al/CFRP tubes.
447
Increasing the number of CFRP plies is also capable of enhancing the energy absorption capacity,
448
while it almost has no improvement on the SEA. The initial loading velocity of the punch
449
significantly affects the crushing force in the early stage, while it has a minor influence on the
450
force in the subsequent stages.
451
(6) Partial CFRP wrapping is an effective approach to increase the crashworthiness of the Al/CFRP
452
tubes. When the plastic deformation region of Al tubes is entirely wrapped by CFRP, the SEA of
453
the hybrid tubes can be increased by 11%. For both constant thickness and constant mass, the
454
multi-cell Al/CFRP tubes outperform their single-cell counterparts in crashworthiness.
17
455
Acknowledgements
456
The present work was supported by National Natural Science Foundation of China (Nos.
457
11672117, 11372115) and Natural Science Fund for Distinguished Young Scholars of Hubei Province.
458
References
459
[1] G. Lu, T. Yu, Energy absorption of structures and materials, Boca Raton : Cambridge : CRC
460
Press ; Woodhead, 2003.
461
[2] A.T. Beyene, E.G. Koricho, G. Belingardi, B. Martorana, Design and Manufacturing Issues in
462
the Development of Lightweight Solution for a Vehicle Frontal Bumper, Procedia
463
Engineering, 88 (2014) 77-84.
464
465
466
467
468
469
470
471
472
473
[3] M. Langseth, O.S. Hopperstad, Static and dynamic axial crushing of square thin-walled aluminium extrusions, Int J Impact Eng, 18 (1996) 949-968. [4] J. Yang, S.R. Reid, Approximate estimation of hardening-softening behaviour of circular pipes subjected to pure bending, Acta Mech Sinica, 13 (1997) 227-240. [5] L. Jing, Z. Wang, J. Ning, L. Zhao, The dynamic response of sandwich beams with open-cell metal foam cores, Compos Part B-Eng, 42 (2011) 1-10. [6] X. Zhang, Z. Wen, H. Zhang, Axial crushing and optimal design of square tubes with graded thickness, Thin-Walled Structures, 84 (2014) 263-274. [7] A. Reyes, M. Langseth, O.S. Hopperstad, Square aluminum tubes subjected to oblique loading, Int J Impact Eng, 28 (2003) 1077-1106.
18
474
[8] M.R. Bambach, H.H. Jama, M. Elchalakani, Static and dynamic axial crushing of spot-welded
475
thin-walled composite steel–CFRP square tubes, International Journal of Impact Engineering,
476
36 (2009) 1083-1094.
477
478
479
480
481
482
483
484
485
486
[9] Z. Huang, X. Zhang, Z. Wang, Transverse crush of thin-walled rectangular section tubes, International Journal of Mechanical Sciences, 134 (2017) 144-157. [10] X.M. Qiu, T.X. Yu, Some Topics in Recent Advances and Applications of Structural Impact Dynamics, Appl Mech Rev, 64 (2012) 030801-030812. [11] X. Zhang, H. Zhang, Z. Wang, Bending collapse of square tubes with variable thickness, Int J Mech Sci, 106 (2016) 107-116. [12] D. Karagiozova, T.X. Yu, G. Lu, Transverse blast loading of hollow beams with square cross-sections, Thin Wall Struct, 62 (2013) 169-178. [13] H. Zhang, X. Zhang, Crashworthiness performance of conical tubes with nonlinear thickness distribution, Thin-Walled Structures, 99 (2016) 35-44.
487
[14] G. Sun, S. Tong, D. Chen, Z. Gong, Q. Li, Mechanical properties of hybrid composites
488
reinforced by carbon and basalt fibers, International Journal of Mechanical Sciences, 148
489
(2018) 636-651.
490
491
[15] G. Zhu, G. Sun, G. Li, A. Cheng, Q. Li, Modeling for CFRP structures subjected to quasistatic crushing, Composite Structures, 184 (2018) 41-55. 19
492
493
[16] D. Kecman, Bending collapse of rectangular and square section tubes, International Journal of Mechanical Sciences, 25 (1983) 623-636.
494
[17] T. Wierzbicki, L. Recke, W. Abramowicz, T. Gholami, J. Huang, Stress profiles in thin-
495
walled prismatic columns subjected to crush loading-II. Bending, Computers & structures,
496
51 (1994) 625-641.
497
498
499
500
501
502
503
504
505
506
507
508
[18] T. Kim, S. Reid, Bending collapse of thin-walled rectangular section columns, Computers & structures, 79 (2001) 1897-1911. [19] Z. Huang, X. Zhang, Three-point bending collapse of thin-walled rectangular beams, International Journal of Mechanical Sciences, 144 (2018) 461-479. [20] Z. Huang, X. Zhang, Three-point bending of thin-walled rectangular section tubes with indentation mode, Thin-Walled Structures, 137 (2019) 231-250. [21] J. Bai, G. Meng, H. Wu, W. Zuo, Bending collapse of dual rectangle thin-walled tubes for conceptual design, Thin-Walled Structures, 135 (2019) 185-195. [22] Z. Wang, Z. Li, X. Zhang, Bending resistance of thin-walled multi-cell square tubes, ThinWalled Structures, 107 (2016) 287-299. [23] J. Obradovic, S. Boria, G. Belingardi, Lightweight design and crash analysis of composite frontal impact energy absorbing structures, Composite Structures, 94 (2012) 423-430.
20
509
[24] A. Rabiee, H. Ghasemnejad, Lightweight design to improve crushing behaviour of multi-
510
stitched composite tubular structures under impact loading, Thin-Walled Structures, 135
511
(2019) 109-122.
512
513
514
515
[25] A. Gliszczyński, L. Czechowski, Collapse of channel section composite profile subjected to bending. Part I: Numerical investigations, Composite Structures, 178 (2017) 383-394. [26] Q. Liu, H. Xing, Y. Ju, Z. Ou, Q. Li, Quasi-static axial crushing and transverse bending of double hat shaped CFRP tubes, Composite Structures, 117 (2014) 1-11.
516
[27] Q. Liu, X. Xu, J. Ma, J. Wang, Y. Shi, D. Hui, Lateral crushing and bending responses of
517
CFRP square tube filled with aluminum honeycomb, Composites Part B: Engineering, 118
518
(2017) 104-115.
519
520
[28] S. Eksi, K. Genel, Bending response of hybrid composite tubular beams, Thin-Walled Structures, 73 (2013) 329-336.
521
[29] Q. Wu, X. Zhi, Q. Li, M. Guo, Experimental and numerical studies of GFRP-reinforced steel
522
tube under low-velocity transverse impact, International Journal of Impact Engineering, 127
523
(2019) 135-153.
524
[30] D.K. Shin, H.C. Kim, J.J. Lee, Numerical analysis of the damage behavior of an
525
aluminum/CFRP hybrid beam under three point bending, Composites Part B: Engineering,
526
56 (2014) 397-407. 21
527
[31] D.-W. Jung, H.-J. Kim, N.-S. Choi, Aluminum–GFRP hybrid square tube beam reinforced by
528
a thin composite skin layer, Composites Part A: Applied Science and Manufacturing, 40
529
(2009) 1558-1565.
530
[32] G. Sun, H. Yu, Z. Wang, Z. Xiao, Q. Li, Energy absorption mechanics and design
531
optimization of CFRP/aluminium hybrid structures for transverse loading, International
532
Journal of Mechanical Sciences, 150 (2019) 767-783.
533
534
535
536
537
538
539
540
[33] Z. Wang, X. Zhang, Z. Li, Bending collapse of multi-cell tubes, International Journal of Mechanical Sciences, 134 (2017) 445-459. [34] ASTM, Standard E8M-04: Standard Test Methods for Tension Testing of Metallic Materials, Testing of Metallic Materials, ASTM, 2004. [35] ASTM, Standard D3039: Standard test method for tensile properties of polymer matrix composite materials (2008). [36] D. ASTM, D695-10: Standard test method for compressive properties of rigid plastics, in, 2010.
541
[37] S. ASTM, D3518. Standard test method for in-plane shear response of polymer matrix
542
composite materials by tensile test of a 45 laminate, in: American Society of Testing
543
Materials, 2001.
22
544
[38] V.S. Sokolinsky, K.C. Indermuehle, J.A. Hurtado, Numerical simulation of the crushing
545
process of a corrugated composite plate, Composites Part A: Applied Science and
546
Manufacturing, 42 (2011) 1119-1126.
547
548
549
550
551
552
553
554
[39] S. Santosa, J. Banhart, T. Wierzbicki, Experimental and numerical analyses of bending of foam-filled sections, Acta Mechanica, 148 (2001) 199-213. [40] Abaqus 6.14, Online Documentation Help, Theory manual: Dassault Systms, Accessed on, (2016). [41] A.F. Johnson, Modelling fabric reinforced composites under impact loads, Composites Part A: Applied Science and Manufacturing, 32 (2001) 1197-1206. [42] P. Maimí, P.P. Camanho, J.-A. Mayugo, C.G. Dávila, A thermodynamically consistent damage model for advanced composites, NASA Technical Report, (2006).
555
23
Figure captions Fig. 1. (a) Representative specimens for the three-point bending tests and (b) dimensions of the sections (units: mm). Fig. 2. Stress-strain curves of: (a) AA6063-O, (b) CFRP in tensile tests, (c) CFRP in compression test, (d) CFRP in in-plane shear test; Test curves for bonding strength between CFRP and CFRP: (e) in normal direction, (f) in shear direction, and test curves for bonding strength between CFRP and Al: (g) in normal direction and (h) in shear direction. Fig. 3. (a) A schematic diagram and (b) the experimental setups for the quasi-static and dynamic impact bending tests. Fig. 4. Typical deformation behaviors of pure CFRP tubes in the quasi-static bending tests and simulations. Fig. 5. Force-displacement curves of the specimens in the quasi-static tests and simulations: (a) CFRP, (b) A2, (c) A4, (d) CA2, (e) CA4 and (f) various specimens. Fig. 6. Deformation processes of double-cell and quadruple-cell Al tubes in the quasi-static tests and simulations: (a) A2 and (b) A4. Fig. 7. Typical deformation behaviors of double-cell and quadruple-cell Al/CFRP tubes in the quasi-static bending tests and simulations: (a) CA2 and (b) CA4. Fig. 8. Final deformed shapes of the specimens in the quasi-static three-point bending tests and simulations: (a) CFRP, (b) A2, (c) A4, (d) CA2 and (e) CA4. Fig. 9. Deformed shapes of the specimens in the dynamic impact tests and simulations: (a) A2, (b) A4, (c) CA2 and (d) CA4. Fig. 10. Comparison of the deformed shapes of the specimens in quasi-static and dynamic impact tests. Fig. 11. Force-displacement curves of tubes in the dynamic three-point bending tests and simulations. Fig. 12. (a) The finite element model of quadruple-cell Al/CFRP tubes under dynamic three-point bending tests and (b) force-displacement curves for different mesh sizes. Fig. 13. Deformed shapes of Al/CFRP tubes with different Al wall thicknesses. Fig. 14. Force-displacement curves of Al/CFRP tubes with different Al wall thicknesses. Fig. 15. Deformed shapes of Al/CFRP tubes with different numbers of CFRP plies. Fig. 16. Force-displacement curves of Al/CFRP tubes with different numbers of CFRP layers. Fig. 17. Deformed shapes of Al/CFRP tubes subjected to different initial velocities. Fig. 18. Force-displacement curves of Al/CFRP tubes subjected to different initial velocities. Fig. 19. Deformed shapes of Al/CFRP tubes with partial CFRP wrapping. Fig. 20. Force-displacement curves of Al/CFRP tubes with partial CFRP wrapping. Fig. 21. Deformed shapes of Al/CFRP tubes with different sectional shapes. Fig. 22. Force-displacement curves of Al/CFRP tubes with different sectional shapes.
Tables Table 1 Energy absorption indices for the specimens under quasi-static three-point bending. Table 2 Energy absorption indices for the specimens under dynamic three-point bending. Table 3 Material properties describing the traction-separation law of cohesive elements. Table 4 Mechanical properties of the CFRP under tensile and compressive loading. Table 5 The parameters for the plastic and failure behaviors of CFRP under shear loading. Table 6 Energy absorption indices for the Al/CFRP tubes with different Al wall thicknesses. Table 7 Energy absorption indices for the Al/CFRP tubes with different numbers of CFRP layers. Table 8 Energy absorption indices for the Al/CFRP tubes under different loading velocity. Table 9 Energy absorption indices for the Al/CFRP tubes with partial CFRP wrapping. Table 10 Energy absorption indices for the Al/CFRP tubes with different sectional shapes.
1
32
1.01
0.95 32
1.01
0.95
(b)
(a)
Fig. 1. (a) Representative specimens for the three-point bending tests and (b) dimensions of the sections (units: mm).
2
(a)
(b)
(c)
(d)
(e)
(f)
(g)
(h)
Fig. 2. Stress-strain curves of: (a) AA6063-O, (b) CFRP in tensile tests, (c) CFRP in compression test, (d) CFRP in in-plane shear test; Test curves for bonding strength between CFRP and CFRP: (e) in normal direction, (f) in shear direction, and test curves for bonding strength between CFRP and Al: (g) in normal direction and (h) in shear direction.
3
(a)
(b)
Quasi-static tests
Impact tests
Drop-hammer test machine
Fig. 3. (a) A schematic diagram and (b) the experimental setups for the quasi-static and dynamic impact bending tests.
4
Fig. 4. Typical deformation behaviors of pure CFRP tubes in the quasi-static bending tests and simulations.
5
(b) A2
(a) CFRP
(c) A4
(d) CA2
(e) CA4
(f) Various specimens
Fig. 5. Force-displacement curves of the specimens in the quasi-static tests and simulations: (a) CFRP, (b) A2, (c) A4, (d) CA2, (e) CA4 and (f) Various specimens.
6
(a) A2
(b) A4
Fig. 6. Deformation processes of double-cell and quadruple-cell Al tubes in the quasi-static tests and simulations: (a) A2 and (b) A4.
7
(a) CA2
(b) CA4
Fig. 7. Typical deformation behaviors of double-cell and quadruple-cell Al/CFRP tubes in the quasi-static bending tests and simulations: (a) CA2 and (b) CA4.
8
(a) CFRP
(b) A2
Simulation
(c) A4
Partial view
Simulation
(d) CA2
Partial view
Simulation
Partial view
(e) CA4
Simulation
Partial view
Simulation
Fig. 8. Final deformed shapes of the specimens in the quasi-static three-point bending tests and simulations: (a) CFRP, (b) A2, (c) A4, (d) CA2 and (e) CA4.
9
(a) A2
Partial view
(b) A4
Simulation
(c) CA2
Partial view
Simulation
Partial view
(d) CA4
Partial view
Simulation
Simulation
Fig. 9. Deformed shapes of the specimens in the dynamic impact tests and simulations: (a) A2, (b) A4, (c) CA2 and (d) CA4.
10
Quasi-static
Dynamic
Quasi-static
Dynamic
Quasi-static
Dynamic
Quasi-static
Dynamic
Fig. 10. Comparison of the deformed shapes of the specimens in quasi-static and dynamic impact tests.
11
Fig. 11. Force-displacement curves of tubes in the dynamic three-point bending tests and simulations.
12
(a)
(b)
Fig. 12. (a) The finite element model of quadruple-cell Al/CFRP tubes under dynamic three-point bending tests and (b) force-displacement curves for different mesh sizes.
13
CA2
t=1.0 mm
CA2
t=1.5 mm
CA2
t=2.0 mm
CA4
t=1.0 mm
CA4
t=1.5 mm
CA4
t=2.0 mm
Fig. 13. Deformed shapes of Al/CFRP tubes with different Al wall thicknesses.
14
Fig. 14. Force-displacement curves of Al/CFRP tubes with different Al wall thicknesses.
15
CA2
layer=3
CA2
layer=5
CA2
layer=7
CA4
layer=3
CA4
layer=5
CA4
layer=7
Fig. 15. Deformed shapes of Al/CFRP tubes with different numbers of CFRP layers.
16
Fig. 16. Force-displacement curves of Al/CFRP tubes with different numbers of CFRP layers.
17
CA2
V=5.1 m/s
CA2
V=15 m/s
CA2
V=25 m/s
CA4
V=5.1 m/s
CA4
V=15 m/s
CA4
V=25 m/s
Fig. 17. Deformed shapes of Al/CFRP tubes subjected to different initial velocities.
18
Fig. 18. Force-displacement curves of Al/CFRP tubes subjected to different initial velocities.
19
CA2
λ=1.0
CA2
λ=0.75
CA2
λ=0.50
CA2
λ=0.25
CA4
λ=1.0
CA4
λ=0.75
CA4
λ=0.50
CA4
λ=0.25
Fig. 19. Deformed shapes of Al/CFRP tubes with partial CFRP wrapping.
20
Fig. 20. Force-displacement curves of Al/CFRP tubes with partial CFRP wrapping.
21
CA1
CA1
t=1.0 mm
m=170.85 g
CA2
CA2
CA4
t=1.0 mm
CA4
m=170.85 g
t=1.0 mm
m=170.85 g
CA9
CA9
Fig. 21. Deformed shapes of Al/CFRP tubes with different sectional shapes.
22
t=1.0 mm
m=170.85 g
Fig. 22. Force-displacement curves of Al/CFRP tubes with different sectional shapes.
23
Table 1 Energy absorption indices for the specimens under quasi-static three-point bending. Stage 1 Section
CFRP-1
Stage 1 + Stage 2
Mass
δ1
E
Pm
SEA
Pm-avg
Pm-simu
Error
δ2
E
Pm
SEA
Pm-avg
Pm-simu
Error
(g)
(mm)
(J)
(kN)
(J/g)
(kN)
(kN)
(%)
(mm)
(J)
(kN)
(J/g)
(kN)
(kN)
(%)
34.75
40.0
16.86
0.42
0.49
/
/
/
/
0.45
0.51
13.3
/
/
/
/
/
/
/
1.92
1.93
0.5
82.8
180.80
2.18
1.68
81.9
174.20
2.13
1.60
2.16
2.18
0.9
2.42
2.46
1.7
85.0
203.10
2.39
1.58
85.0
204.40
2.40
1.59
2.40
2.36
-1.7
85.0
235.10
2.77
1.65
2.45
2.48
1.2
85.0
233.70
2.75
1.64
2.76
2.71
-1.8
3.39
3.15
-7.1
85.0
278.60
3.28
1.70
85.0
275.60
3.24
1.68
3.26
3.10
-4.9
CFRP-2
35.23
40.0
19.19
0.48
0.54
A2-1
107.87
45.0
85.68
1.90
0.79
A2-2
108.76
45.0
87.32
1.94
0.80
A4-1
128.58
45.0
109.14
2.43
0.85
A4-2
128.70
45.0
107.99
2.40
0.84
CA2-1
142.78
45.0
112.71
2.50
0.79
CA2-2
142.90
45.0
107.79
2.40
0.75
CA4-1
164.01
45.0
157.05
3.49
0.96
CA4-2
164.31
45.0
148.23
3.29
0.90
24
Table 2 Energy absorption indices for the specimens under dynamic three-point bending. Stage 1 Section
A2-1
Mass
δ1
E
Pm
SEA
Pm-avg
Pm-simu
Error
δ2
E
Pm
SEA
Pm-avg
Pm-simu
Error
(g)
(mm)
(J)
(kN)
(J/g)
(kN)
(kN)
(%)
(mm)
(J)
(kN)
(J/g)
(kN)
(kN)
(%)
106.98
45.0
98.03
2.18
0.92
85.0
190.62
2.24
1.78
2.19
2.16
-1.4
85.0
175.68
2.07
1.63
2.16
2.23
3.2
2.79
2.81
0.7
85.0
229.49
2.71
1.78
85.0
232.64
2.76
1.80
2.74
2.90
5.8
2.45
2.66
8.6
85.0
226.60
2.67
1.59
85.0
218.17
2.57
1.52
2.62
2.71
3.4
85.0
296.65
3.49
1.80
3.47
3.29
-5.2
85.0
296.99
3.49
1.81
3.49
3.25
-6.9
A2-2
107.72
45.0
98.73
2.19
0.92
A4-1
129.07
45.0
126.18
2.80
0.98
A4-2
129.26
45.0
124.88
2.78
0.97
CA2-1
142.28
45.0
107.01
2.38
0.75
CA2-2
143.83
45.0
113.18
2.52
0.79
CA4-1
164.65
45.0
155.98
3.47
0.95
CA4-2
Stage 1 + Stage 2
164.50
45.0
155.93
3.47
0.95
25
Table 3 Material properties describing the traction separation law of cohesive elements.
Elastic properties (MPa)
Variable
Delamination
Debonding
Kn
1000
1000
Ks
1000
1000
Kt
1000
1000
0
4.8
3.4
0
14.8
9.4
tt0
tn Damage initiation (MPa)
ts
14.8
9.4
c
202
143
c
891
566
Gtc
891
566
η
2.284
2.284
Gn 2
Fracture energies (J/m )
BK
Gs
26
Table 4 Mechanical properties of the CFRP under tensile, compressive and in-plane loading.
3
Density (kg/m )
Elastic properties (GPa)
Damage initiation (MPa)
2
Fracture energies (kJ/m )
27
Variable
Value
ρ
1320
E1
42.7
E2
42.7
G12
4.4
v12
0.05
X1+
643
X1-
267
X2+
643
X2-
267
S
37
Gfc1+
83
Gfc1-
72
Gfc2+
83
Gfc2-
72
Table 5 The parameters for the plastic and failure behaviors of CFRP under shear loading. Coefficient in the shear damage variable Maximum value of shear damage variable
β12
0.18
d12max
0.99
^
Initial effective shear yield stress (MPa)
σy0
58
Power term in the hardening equation
C
1053
Coefficient in the hardening equation
P
0.41
28
Table 6 Energy absorption indices for the Al/CFRP tubes with different Al wall thicknesses. Stage 1 Section
Stage 1 + Stage 2
t
Mass
δ1
E
Pm
SEA
δ2
E
Pm
SEA
(mm)
(g)
(mm)
(J)
(kN)
(J/g)
(mm)
(J)
(kN)
(J/g)
CA2
1.0
148.25
40
113.93
2.85
0.77
80
223.15
2.79
1.51
CA2
1.5
204.75
40
174.33
4.36
0.85
80
319.13
3.99
1.56
CA2
2.0
261.25
40
287.91
7.19
1.10
80
464.07
5.80
1.76
CA4
1.0
170.85
40
133.42
3.34
0.78
80
257.17
3.21
1.51
CA4
1.5
238.65
40
222.59
5.56
0.93
80
376.26
4.70
1.58
CA4
2.0
306.45
40
320.78
8.02
1.05
80
548.17
6.85
1.78
29
Table 7 Energy absorption indices for the Al/CFRP tubes with different numbers of CFRP plies. Stage 1 Section
Layer
Stage 1 + Stage 2
Mass
δ1
E
Pm
SEA
δ2
E
Pm
SEA
(g)
(mm)
(J)
(kN)
(J/g)
(mm)
(J)
(kN)
(J/g)
CA2
3
148.25
40
113.93
2.85
0.77
80
223.15
2.79
1.51
CA2
5
171.75
40
140.12
3.50
0.82
80
262.86
3.28
1.53
CA2
7
195.25
40
167.75
4.19
0.86
80
311.46
3.89
1.60
CA4
3
170.85
40
133.42
3.34
0.78
80
257.17
3.21
1.51
CA4
5
194.35
40
159.67
3.99
0.82
80
297.05
3.71
1.53
CA4
7
217.85
40
180.39
4.51
0.83
80
337.38
4.22
1.55
30
Table 8 Energy absorption indices for the Al/CFRP tubes under different loading velocity. Stage 1 Section
Stage 1 + Stage 2
V
Mass
δ1
E
Pm
SEA
δ2
E
Pm
SEA
(mm)
(g)
(mm)
(J)
(kN)
(J/g)
(mm)
(J)
(kN)
(J/g)
CA2
5.1
148.25
40
113.93
2.85
0.77
80
223.15
2.79
1.51
CA2
15
148.25
40
131.63
3.28
0.89
80
247.89
3.10
1.67
CA2
25
148.25
40
139.11
3.48
0.94
80
266.52
3.33
1.80
CA4
5.1
170.85
40
133.42
3.34
0.78
80
257.17
3.21
1.51
CA4
15
170.85
40
152.36
3.80
0.89
80
293.13
3.66
1.72
CA4
25
170.85
40
166.26
4.15
0.97
80
307.51
3.84
1.80
31
Table 9 Energy absorption indices for the Al/CFRP tubes with partial CFRP wrapping. Stage 1 Section
λ
Stage 1 + Stage 2
Mass
δ1
E
Pm
SEA
δ2
E
Pm
SEA
(g)
(mm)
(J)
(kN)
(J/g)
(mm)
(J)
(kN)
(J/g)
CA2
1.00
148.25
40
113.93
2.85
0.77
80
223.15
2.79
1.51
CA2
0.75
139.44
40
113.61
2.84
0.81
80
220.21
2.75
1.58
CA2
0.50
130.63
40
111.88
2.80
0.86
80
213.29
2.67
1.63
CA2
0.25
121.81
40
99.07
2.47
0.81
80
154.69
1.93
1.27
CA4
1.00
170.85
40
133.42
3.34
0.78
80
257.17
3.21
1.51
CA4
0.75
162.04
40
132.87
3.32
0.82
80
257.05
3.21
1.59
CA4
0.50
153.23
40
132.41
3.31
0.87
80
256.42
3.20
1.67
CA4
0.25
144.41
40
121.04
3.02
0.84
80
220.67
2.76
1.53
32
Table 10 Energy absorption indices for the Al/CFRP tubes with different sectional shapes. Stage 1 Section
Stage 1 + Stage 2
t
Mass
δ1
E
Pm
SEA
δ2
E
Pm
SEA
(mm)
(g)
(mm)
(J)
(kN)
(J/g)
(mm)
(J)
(kN)
(J/g)
CA1
1.00
125.65
40
89.03
2.23
0.71
80
174.78
2.18
1.39
CA2
1.00
148.25
40
113.93
2.85
0.77
80
223.15
2.79
1.51
CA4
1.00
170.85
40
133.42
3.34
0.78
80
257.17
3.21
1.51
CA9
1.00
216.05
40
200.85
5.02
0.93
80
397.09
4.96
1.84
CA1
1.48
170.85
40
134.37
3.36
0.79
80
212.06
2.65
1.24
CA2
1.19
170.85
40
125.94
3.15
0.74
80
244.97
3.06
1.43
CA4
1.00
170.85
40
133.42
3.34
0.78
80
257.17
3.21
1.51
CA9
0.76
170.85
40
147.69
3.69
0.86
80
304.53
3.81
1.78
33
Highlights (1) Quasi-static and dynamic three-point bending tests are conducted for Al/CFRP tubes; (2) Numerical analyses are performed to simulate the tests and analyze the mechanisms; (3) The bending responses and energy absorption performances of tubes are analyzed; (4) The influences of various factors on the bending responses of tubes are investigated; (5) The multi-cell Al/CFRP tubes outperform the single-cell counterparts in crashworthiness.
Declaration of interests