Nanoindentation study of the interfacial zone between cellulose fiber and cement matrix in extruded composites

Nanoindentation study of the interfacial zone between cellulose fiber and cement matrix in extruded composites

Accepted Manuscript Nanoindentation study of the interfacial zone between cellulose fiber and cement matrix in extruded composites R.S. Teixeira, G.H...

3MB Sizes 3 Downloads 35 Views

Accepted Manuscript Nanoindentation study of the interfacial zone between cellulose fiber and cement matrix in extruded composites R.S. Teixeira, G.H.D. Tonoli, S.F. Santos, E. Rayon, V. Amigó, H. Savastano, Jr., F.A. Rocco Lahr PII:

S0958-9465(16)30464-4

DOI:

10.1016/j.cemconcomp.2017.09.018

Reference:

CECO 2916

To appear in:

Cement and Concrete Composites

Received Date: 19 August 2016 Revised Date:

14 July 2017

Accepted Date: 29 September 2017

Please cite this article as: R.S. Teixeira, G.H.D. Tonoli, S.F. Santos, E. Rayon, V. Amigó, H. Savastano Jr., F.A.R. Lahr, Nanoindentation study of the interfacial zone between cellulose fiber and cement matrix in extruded composites, Cement and Concrete Composites (2017), doi: 10.1016/ j.cemconcomp.2017.09.018. This is a PDF file of an unedited manuscript that has been accepted for publication. As a service to our customers we are providing this early version of the manuscript. The manuscript will undergo copyediting, typesetting, and review of the resulting proof before it is published in its final form. Please note that during the production process errors may be discovered which could affect the content, and all legal disclaimers that apply to the journal pertain.

1

ACCEPTED MANUSCRIPT Nanoindentation study of the interfacial zone between cellulose fiber and

2

cement matrix in extruded composites

3 4

R.S. Teixeira1; G.H.D. Tonoli2; S.F. Santos3, E. Rayon4, V. Amigó4; H. Savastano Jr5; F.A.

5

Rocco Lahr1. 1

University of São Paulo (USP), Department of Structural Engineering. School of Engineering of São Carlos, Brazil; 2 Federal University of Lavras (UFLA), Department of Forest Science, Brazil; 3 São Paulo State Universit (UNESP), School of Engineering, Department of Materials and Technology, Brazil; 4 Universitat Politècnica de València (UPV), Department of Mechanical and Materials Engineering, Spain. 5 University of São Paulo (USP), Department of Biosystems Engineering, Brazil.

15

ABSTRACT

16

The present study shows the application of the nanoindentation technique to evaluate the

17

properties of the cellulose fiber-cement matrix interfacial zone in composites prepared with an

18

auger extruder. The degree of strength of the bond between fiber and matrix is recognized as

19

important variable that influences macro-mechanical properties, such as modulus of rupture

20

and toughness of cement based composites. The nanoindentation measurements showed the

21

highest hardness and elastic modulus in the part inner of the cellulosic fiber after hydration

22

process due to precipitation and re-precipitation of cement hydration products. These results

23

indicate that mineralization of the cellulosic fibers can affect the stress distribution and

24

interfacial bond strength in the cement based composite.

TE D

M AN U

SC

RI PT

6 7 8 9 10 11 12 13 14

EP

25

KEYWORDS: vegetable fiber, microstructure, mechanical properties, ordinary Portland

27

cement, transition zone.

28

AC C

26

29

1 INTRODUCTION

30

It is widely accepted that concrete at the mesoscopic scale should be treated as a three-phase

31

composite material constituted by bulk hardened cement paste, aggregates and an interfacial

32

transition zone (ITZ) between these two. [1] Therefore, traditional ITZ is the region of the

33

cement matrix around the aggregate particles, which is perturbed by the presence of the

34

aggregate. Its origin lies in the packing of the cement grains against the much larger

35

aggregate, which leads to a local increase in porosity and predominance of smaller cement

36

particles in this region. The ITZ is region of gradual transition and is highly heterogeneous,

37

nevertheless the average microstructural features may be measured [2].

ACCEPTED MANUSCRIPT

The cementitious composites reinforced with cellulosic fibers are complex materials. Thus,

39

cement based composite design must be considered for the interrelation between interfacial

40

transition zone, fibers, matrix and processing method. Particle and fiber size distribution,

41

particles and fibers packing and rheological behavior of the cement paste with fibers in the

42

fresh state also interfere on the interfacial transition zone of the hardened cement based

43

composite. Furthermore, changes in the mechanical properties over time can occur due to

44

microstructural changes in the fiber-matrix interface and bulk, as a consequence of the

45

continued hydration process that occurs in the fiber surroundings, i.e. if the interfacial

46

transition zone becomes denser due to re-precipitation of cement hydration products in the

47

porous layers. [3]. Therefore, in this manuscript an interfacial transition zone (ITZ)

48

terminology is related to a region between bulk hardened cement paste and cellulosic fiber.

49

Kraft pulp fiber-reinforced cement-based materials have being increasingly used in most

50

developing countries as construction materials [4–6]. Fibers usually increase mechanical

51

strength and the capacity of cement based composite to absorb energy through the distribution

52

of microcracks into the material. The bonding between cellulose fiber and Portland cement

53

plays a major role in the transference of the load from the matrix to the reinforcement,

54

impacting the mechanical behavior of the resulting fiber-cement material. This bonding can

55

be of physical (mechanical interlocking) or chemical (mainly hydrogen bonds) nature, or a

56

combination of both [7].

57

Extrusion process has a potential of producing fiber reinforced cementitious composites with

58

higher performance compared to the traditional slurry dewatering processes such as Hatschek

59

and Flow-on methods. Several advantages of extrusion moulding can be pointed for

60

manufacturing of fibrous composites: (i) low implementation cost; (ii) low capillary porosity

61

of extruded composites; and (iii) low water/cement ratio, which plays a significant role for

62

improving of the fiber-matrix interface zone [8–10]. As mentioned above, the control of fiber-

63

matrix interface zone in extruded composites depends on cellulosic fibers and matrix

64

constituent’s properties, cure procedure as well as weathering conditions that the composite

65

are exposed. Previous studies highlighted that water/cement ratio influences the interface zone

66

thickness and that lower porosity may increase composite strength and matrix toughness [9–

67

12]. Therefore, the optimization of the interfacial zone is not an easy task since it is necessary

68

to satisfy the equilibrium between fiber-matrix adhesion and fiber pull-out. In addition, there

69

is still a lack of information about the consequences of the different types of interface zone

70

between cellulose fibers and matrix, on composite mechanical properties. Thus, an effort is

71

required in order to understand the mechanical properties at fiber-matrix transition zone.

AC C

EP

TE D

M AN U

SC

RI PT

38

ACCEPTED MANUSCRIPT

The macroscale mechanical properties of bulk materials are dependent on the properties of

73

their microscale/nanoscale constituents and the interface between these constituents.

74

Microindentation technique is one of the developing tests that have been used for evaluating

75

mechanical characteristics of microsized zones in diverse cement based composites [13–15].

76

Nevertheless, microindentation is not capable to detect mechanical differences at the

77

interfaces between cement matrix and reinforced fibers, due to some limitations, such as a

78

resolution of microindentation system in terms of load is about 5.0 mN, to analyze some

79

structural features because of the heterogenity of the specimen, inadequate spacing between

80

indents or form edges, operator’s visual acuity. Quasistatic nanoindentation has become the

81

standard technique used for nanomechanical characterization of small volumes of material,

82

such as elastic modulus, hardness at the nanoscale. It is used machines that can record small

83

load and displacement with high accuracy and precision, during loading and unloading can be

84

continuously monitored with high resolution in the nanonewton and nanometer ranges. In this

85

technique is used usually the Berkovich tip is a 3-sided pyramid that have an apex appropriate

86

for investigating the interface transition zone between fiber and matrix. Therefore,

87

nanoindentation technique can contribute to quantitatively measure the underlying source of

88

the bulk response at the nanoscale in cement based composites that are heterogeneous

89

material from both a chemical composition and nanoscale structure standpoint. Being able to

90

evaluate at this scale allows micro and nano structural "tuning" to be performed to optimize

91

bulk properties [16,17]. The aim of this study was to evaluate the interfacial zone between

92

fibers to cement matrix in extruded composites reinforced with eucalyptus pulp, using a

93

nanoindentation technique allied with microscopic examinations.

94

EP

TE D

M AN U

SC

RI PT

72

2 EXPERIMENTAL

96

2.1 Materials

97

Unbleached unrefined eucalyptus (Eucalyptus grandis) Kraft pulp was provided by Fibria

98

S/A, Brazil. The cellulose pulp was collected directly from the mill, prior to drying and

99

pressing. It was extensively washed with water and centrifuged to remove any residual

AC C

95

100

chemicals from the pulping processes.

101

Eucalyptus pulps were analyzed about morphology (length and width) and concentration of

102

particles (fibers per gram and content of fines). A fine element (small particles with length

103

lower than 200 µm that are commonly called fines, which also contain band-like materials

104

from both primary wall and secondary wall layers of the fibers) was detected in the pulp with

105

dimensions lower than those of fibers. Fines do not contribute significantly to cement based

ACCEPTED MANUSCRIPT

106

composite strength but act more as filler [18]. Physical characteristics of the unbleached

107

eucalyptus pulp are showed in Table 1.

108 2.2 Composite mix design

110

Formulation used in the composite production was based on previous study [8], and is

111

described in Table 2.

112

Portland cement and limestone particles distribution was performed by laser particle size

113

analyzer (Malvern Mastersizer S long bed, version 2.19). Cement and limestone particles

114

showed 50% of their size below 11 µm and 16 µm respectively.

115

Hydroxypropylmethylcellulose (HPMC) from Aditex, is a superplasticizer which disperses

116

cement particles, reducing the flow stress and the viscosity of the cement paste. Polyether

117

carboxylic provided by Grace, commercially called ADVA 170, is an additive which reduces

118

the surface tension of the water and thus causes an increase in the surface area of the liquid

119

which improves the water absorption, forming a lubrication layer between the wall of the

120

extruder and the surface of the fiber cement board. HPMC with 86,000 average molecular

121

weight and 5.39 cPs viscosity (at 2% concentration in water at 20°C) and polyether carboxylic

122

commercially named ADVA 170, were used as rheological modifiers in fiber-cement, with

123

dosage of 1 wt% of the total mass of the particulate inorganic materials (Portland cement and

124

limestone) to promote the pseudo-plastic behavior of the composite, which, in turn, enabled

125

the extrusion process.

126

TE D

M AN U

SC

RI PT

109

2.3 Composite extrusion

128

The mass was mixed in a mechanical Eirich intensive mixer (capacity of 10 L) for 5 min at

129

125 rpm, 5 min at medium velocity (220 rpm) and finally 5 min at high velocity (450 rpm).

130

The water-cement (w/c) ratio was 0.33. The composite mixture was transferred to a Verdes

131

051 extruder (Figure 1a-b). The speed of the extruder was 4 mm/s; die width/diameter ratio

132

was 3.3. Composites were molded in 15 mm x 50 mm x 200 mm plates. The illustration of the

133

chamber parts of the extruder is presented in Figure 1c.

134

The composite mixture was re-circulated into the extruder for 5 min before tailoring the

135

samples. Pads with 15 mm x 50 mm x 200 mm were cured at water vapor saturated

136

environment (in sealed plastic bags) at 25 ± 2ºC for two days. Subsequently, the specimens

137

were maintained in water vapor saturated environment (in sealed plastic bags) and placed in a

138

chamber at 45ºC for five days (thermal curing) totalizing 7 days of cure [21].

139 140

AC C

EP

127

ACCEPTED MANUSCRIPT

2.4 Microstructure characterization

142

The specimens were cut out from the middle section of a larger volume of fiber cement, with

143

minimal deformation, by using a precision cutter, Buehler, model Isomet, with precision

144

diamond saw, 15LC, and using an isopropyl alcohol based cutting fluid to cut. This method

145

provides roughness smaller. The specimens were embedded in epoxy resin (MC-

146

DUR1264FF) previously to be visualized in a scanning electron microscope (SEM). A final

147

polishing was carried out using sequentially 8-4 µm, 4-2 µm and 1-0 µm diamond abrasives,

148

as reported elsewhere [22,23]. The polished samples were carbon coated before being

149

analyzed in a JEOL JSM6300 electron microscope with acceleration voltage of 20 kV. A

150

back-scattered electron (BSE) detector was used to observe the morphological features on the

151

cross-section and polished surfaces. BSE imaging permits the identification of cementitious

152

phases since the electron scattering change. Dark and light areas are related to lighter and

153

heavier elements respectively. Energy dispersive spectrometry (EDS) analysis was performed

154

in order to identify the chemical composition in different spots on the same polished surface

155

specimens.

M AN U

SC

RI PT

141

156

2.4.1 Atomic force microscopy characterization (AFM)

158

In contrast to ductile material, cement based composite have regions with higher hardness,

159

lower ductility, and a basically brittle nature. Due to the brittleness, cellulosic fibers and

160

porosity of the composite it is quite often difficult to cut and polish. All areas of the

161

specimens observed by nanoindentation were cut and polished with uniformity and carefully

162

to avoid any pullout of fibers, but as the composite is heterogeneous the response of each

163

region was different according to its resistance. Specimens for AFM characterization were cut

164

with same system mentioned above and embedded in polyacrylamide. The semi-automatic

165

polisher was used to adjust polishing velocity and pressure, i.e. all regions were submitted to

166

same conditions of preparation. Then, the dried surfaces were grinded in a sequence of SiC

167

papers (grit #500, #1000, #2000 and #4000) and polished in a cloth sequentially with 9 µm,

168

6 µm and 3 µm diamond sprays. Finally, the specimen surfaces were cleaned by washing in

169

alcohol and ultrasonic bathing.

170

The characterization of the fiber-matrix interface zone was carried out using the tapping-mode

171

atomic force microscopy (TM-AFM) to obtain height and phase imaging data simultaneously,

172

with Nanoscope III-Digital Instruments. Silicon cantilever with spring constant of around

173

70 N/m and a scan area of 15 µm x 15 µm was used. Samples were prepared in the laboratory

174

environment with temperature around 25°C and relative humidity between 50% and 65%.

AC C

EP

TE D

157

ACCEPTED MANUSCRIPT

175

AFM images were obtained in the same laboratory environment conditions. The test locations

176

were guided by means of an incorporated optical light microscope.

177 2.5 Nanoindentation tests

179

Specimens for nanoindentation tests were prepared the same methodology that specimens to

180

AFM characterizations. Nanoindentation was performed in an Agilent G-200 instrument

181

working in continuous stiffness measurement (CSM), configured at 2 nm of harmonic

182

amplitude, 45 Hz frequency, and using a Berkovich indenter. The test locations were guided

183

by means of an incorporated optical light microscope. To rule out the influence of surface

184

morphology, the indentation depth should be much greater than the characteristic size of

185

surface roughness to avoid errors and size effect in the calculations [17]. Tests were

186

programmed to reach from 100 to 300 nm-indented depths until the maximum depth of 1000

187

nm. Therefore, the depth of the imprint spots used in the nanoindentation was to minimize

188

surface roughness of the samples. Analyses were performed with 8 nm distance between the

189

measurement points [17]. It was performed more than 20 analyses for each region of the

190

composite (bulk matrix, interface or transition zone, anhydrous grain and cellulose fibers).

191

To guarantee a significance results for nanoindentation tests were choose under a completely

192

randomized design the ITZ areas to analyze a linear sequence with four regions (transition

193

zone, cellulose fiber, transition zone, bulk matrix and anhydrous grain or follow sequence:

194

anhydrous grain, bulk matrix, cellulose fiber, transition zone) and twenty replications. The

195

effects of hardness and elastic modulus were compared via statistical contrast by student test

196

at 5% of significance [17]. The ACTION statistical program was used. Therefore, the

197

interfaces towards fibers and matrix were studied in greater detail.

SC

M AN U

TE D

EP

198

RI PT

178

3 RESULTS AND DISCUSSION

200

3.1 Chemical and microstructure characterization

201

Figure 2 shows SEM-BSE micrographs of the extruded composites. Energy dispersive X-ray

202

spectroscopy (EDS) analysis (Figure 2a) indicate that fiber-matrix interfacial zone presents

203

high Ca/Si ratio (between 4 to 5), indicating the possible correspondence with Ca(OH)2

204

crystals with carbonated products, such as calcite, as corroborated by AFM analysis (Figure

205

3) and according to Ruiz-Agudo et al. [24]. This interfacial zone rich in Ca(OH)2 crystals has

206

been widely reported in literature for cementitious composites [25–29]. Bulk matrix revealed

207

an expected lower Ca/Si ratio (approximately 2.5) as observed in Figure 2b. The phase

208

composition of the anhydrous grains and matrix are shown in Figures 4a and 4b, respectively.

209

Spot B presents higher concentration of SiO2 and CaO due to the hydration products of

AC C

199

210

ACCEPTED MANUSCRIPT

cement in relation to the spot A (region of the anhydrous grain).

211 3.2 Mechanical characterization by nanoindentation

213

Figures 5a and 6a present the micrographs of the nanoindentation imprints done along the

214

bulk section of the composites. The spots numbered between 1-10 (Figure 5a), 25-61 (Figure

215

5a) and 81-90 (Figure 6a) represent the bulk matrix of the composite. The spots 15-16 (Figure

216

5a), 20-22 (Figure 5a) and 101-110 (Figure 6a) represents the interfacial zone. The spots 16-

217

19 (Figure 5a) and 91-100 (Figure 6a) represents the cellulosic fiber, while 62-70 (Figure 5a)

218

and 81-90 (Figure 6a) are spots related to anhydrous grains. The individual values of elastic

219

modulus (E) acquired for each spot are summarized in Figures 5b and 6b; while the individual

220

values of hardness (H) is presented in Figures 5c and 6c.

221

Table 3 shows the average and standard deviation values of elastic modulus and hardness

222

obtained from nanoindentation in the different regions studied. The indent spots in the bulk

223

matrix led to elastic modulus of around 70 GPa and hardness of around 5 GPa. These results

224

are similar to those found by Silva et al. [17], who studied nanoindentation in concrete

225

specimens. The bulk matrix of composites based on Portland cement normally presents

226

calcium silicate hydrates (C-S-H) and calcite phases as main components, which have higher

227

rigidity and relative lower porosity than other phases such as Ca(OH)2 and ettringite that are

228

formed by poorly packed structures. This is why the spots correspondent to the

229

interfacial/transition zone presents lower elastic modulus (~17 GPa) and hardness (~0.4 GPa).

230

These results of the elastic modulus and hardness vary in relation to the distance of the

231

transition zone, as showed in Figure 5. Similar result was found by Wang et al. [30] that

232

studied nanoindentation technique in concrete reinforced with steel fibers. The values of

233

hardness in the 11-12, 23-26 indent spots near to the interfacial zone are smaller than those in

234

the matrix region, which are also related to the higher porosity in the interfacial zone,

235

resultant of the low adhesion between fiber and matrix [31,32].

236

Other important observation from this study in nanoscale level is related to the hydration of

237

the cement grains in the composite. The incorporation of water during the mixing of the

238

composite constituents leads to cement hydrate grains that have much lower average atomic

239

numbers than cement grains that were not completely hydrated (anhydrous grains). Then,

240

strong contrast is obtained between unreacted (anhydrous) and reacted material (hydrates)

241

[33]. Anhydrous grain shown in Table 3 presents elastic modulus of around 90.0 GPa and

242

hardness of around 4.5 GPa, which was not significantly different from average values of

243

hydrated bulk matrix. Velez et al. [34] also studied nanoindentation in cement and did not

AC C

EP

TE D

M AN U

SC

RI PT

212

ACCEPTED MANUSCRIPT

find differences between hardness and elastic modulus in anhydrous phases such as alite

245

(C3S), calcium aluminate (C3A) and belite (C2S).

246

The highly alkaline pore water within the fiber-cement interface can induce the cellulose

247

fibers stiffening. It occurs because cellulose fibers are hydrophilic and absorb water rich in

248

cement hydration products, leading to the mineralization phenomenon proposed elsewhere

249

[35–37]. This phenomenon is related to hydrophilic nature of the cellulose fibers. Therefore,

250

this phenomenon is related to the hydrophilic nature of the cellulose fibers. This nature

251

depends on surface nature, surface porosity and lumens the inner of the cellulose fiber. The

252

internal humidity in the fiber can promote a continued hydration process, with precipitation

253

and re-precipitation internally, such as C-S-H, portlandite and calcites, as suggest by Figures

254

7a and 7b. Figure 7a shows hydration products within the cell wall of cellulosic fibers, while

255

the EDS spectra (Figure 7b) in the spots 1 (upper) and 2 (bottom) proves the large amounts of

256

Si and Ca into the cellulose fibers. It explains the higher values of elastic modulus (~144 GPa)

257

and hardness (~9 GPa) observed for the nanoindentation spots related to the cellulosic fiber

258

regions. Therefore, the average elastic modulus of mineralized cellulose fibers can reach

259

higher values than cement bulk matrix. The increase of stiffness of the cellulose fibers is a

260

drawback because can induce the loss of their reinforcement capacity. The efficiency of stress

261

transfer from matrix to fiber that is of fundamental importance in determining the mechanical

262

properties of short fibre reinforced composite is prejudiced. This result explain the premature

263

loss of ductility/toughness and increase of stiffness of composites reinforced with cellulose

264

fibers widely reported in literature [22,23,38,39].

265

Therefore, the fiber to matrix bonding is impaired because cellulose fiber tends to exchange

266

water with the matrix system by capillary action, leading to high dimensional variation and

267

detachment of the fiber surface from the matrix, as showed in Figure 7a, creating voids that

268

explain the low results of elastic modulus and hardness in the transition zone. Finally, the

269

present observations may state that an optimal situation would be the cellulose fibers

270

protection from excessive water absorption, what can be achieved by less hydrophilic surfaces

271

(either natural or after an adequate treatment) and without losing the fiber bridging. Fiber

272

bridging is important to guarantee the expend of energy during fiber pullout, which leads to

273

composite ductility.

AC C

EP

TE D

M AN U

SC

RI PT

244

274 275

4 CONCLUSIONS

276

High values of elastic modulus and hardness, 144 ± 48.9 GPa and 9 ± 2.5 GPa, respectively,

277

was found by means of nanoindentation imprints in the cellulose fiber, because of the

278

majority presence of C-S-H, portlandite and calcite phases. Then, cellulose fibers absorb

ACCEPTED MANUSCRIPT

water rich in cement hydration products, which induce the cellulose fiber stiffening by the

280

precipitation and re-precipitation of hydration products into the fiber, these phenomenon lead

281

to the so-called mineralization process. The increase of stiffness of the inner part of the

282

cellulose fibers is a drawback because can induce the loss of their reinforcement capacity. .

283

The present finding contributes to better understanding the interface properties between fiber

284

and matrix that affect cellulose fiber-cement materials performance, in terms of macroscopic

285

mechanical properties. It is difficult to obtain the effective elastic modulus these composites

286

because the low adhesion between the hydrophilic cellulose fibers and cement matrix,

287

mineralization of the cellulose fiber and consequently a significant difference of elastic

288

modulus between matrix, interface transition zone (ITZ), and cellulose fiber. These results

289

indicate a clear modification of the contribution of the cellulosic fiber in the stress distribution

290

and interfacial bond strength in the cement based composite. Therefore, it is still a challenge

291

to modify nano and micro structures of the ITZ in order to improve mechanical properties in

292

macro scale of the extruded fiber-cement composites.

293

M AN U

SC

RI PT

279

5 ACKNOWLEDGEMENTS

295

The authors acknowledge by financial support provided by Fundação de Amparo à Pesquisa

296

do Estado de São Paulo (FAPESP, process nº 2013/03823-8), Coordenação de

297

Aperfeiçoamento de Pessoal de Nível Superior (CAPES, process nº 3886/2014) and Conselho

298

Nacional de Desenvolvimento Científico e Tecnológico (CNPq), in Brazil. Special thanks for

299

Fibria and Infibra for providing raw materials the development of this work.

302 303 304 305 306 307 308 309 310 311 312 313

EP

301

AC C

300

TE D

294

ACCEPTED MANUSCRIPT

314

6 REFERENCES

315

[1]

316

in simulated cement microstructures, Cem. Concr. Compos. 80 (2017) 224–234.

317

doi:10.1016/j.cemconcomp.2017.03.008.

318

[2]

319

between cement paste and aggregate in concrete, Interface Sci. 12 (2004) 411–421.

320

doi:10.1023/B:INTS.0000042339.92990.4c.

321

[3]

322

lignocellulosic fiber and matrix in cement-based composites, Editors: Holmer Savastano

323

Junior, Juliano Fiorelli and Sergio Francisco dos Santos, Woodhead Publishing, 2017, pp. 27-

324

68. doi:10.1016/j.actamat.2015.02.029.

325

[4]

326

new high toughness polypropylene (PP) fibers in air-cured Hatschek process, Constr. Build.

327

Mater. 24 (2010) 171–180. doi:10.1016/j.conbuildmat.2009.06.019.

328

[5]

329

carbonation on cementitious roofing tiles reinforced with lignocellulosic fibre, Constr. Build.

330

Mater. 24 (2010) 193–201. doi:10.1016/j.conbuildmat.2007.11.018.

331

[6]

332

Eucalyptus pulp fibres as alternative reinforcement to engineered cement-based composites,

333

Ind. Crops Prod. 31 (2010) 225–232. doi:10.1016/j.indcrop.2009.10.009.

334

[7]

335

R.N. (Ed.), Nat. Fibre Reinf. Cem. Concr., Glasgow: Blackie,1988. pp.208-42. (Concrete

336

Technology and Design, 5), 1988.

337

[8]

338

Extruded Cement Based Composites Reinforced with Sugar Cane Bagasse Fibres, Key Eng.

339

Mater. 517 (2012) 450–457. doi:10.4028/www.scientific.net/KEM.517.450.

340

[9]

341

8 (1973) 352–362. doi:10.1007/BF00550155.

342

[10]

343

extrusion, Can. J. Civ. Eng. 27 (2000) 543–552. doi:10.1139/cjce-27-3-543.

344

[11]

345

composites, Cem. Concr. Compos. 21 (1999) 49–57. doi:10.1016/S0958-9465(98)00038-9.

346

[12]

347

cement components for roofing, Constr. Build. Mater. 13 (1999) 433–438.

348

doi:10.1016/S0950-0618(99)00046-X.

P. Carrara, L. De Lorenzis, Consistent identification of the interfacial transition zone

RI PT

K.L. Scrivener, A.K. Crumbie, P. Laugesen, The interfacial transition zone (ITZ)

SC

S.F. Santos, R.S. Teixeira, H. Savastano Jr., Interfacial transition zone between

M AN U

S. Ikai, J.R. Reichert, A. V. Rodrigues, V.A. Zampieri, Asbestos-free technology with

G.H.D. Tonoli, S.F. Santos, A.P. Joaquim, H. Savastano Jr, Effect of accelerated

TE D

G.H.D. Tonoli, H. Savastano, E. Fuente, C. Negro, A. Blanco, F.A. Rocco Lahr,

EP

R.S.P. COUTTS, Wood fibre reinforced cement composites., in: (Ed.) In: SWAMY,

AC C

R.S. Teixeira, G.H.D. Tonoli, S.F. Santos, J. Fiorelli, H. Savastano Jr., F.A.R. Lahr,

J. Aveston, A. Kelly, Theory of multiple fracture of fibrous composites, J. Mater. Sci.

Y. Shao, S. Moras, N. Ulkem, G. Kubes, Wood fibre - cement composites by

H. Savastano Jr, V. Agopyan, Transition zone studies of vegetable fibre-cement paste

H. Savastano Jr, V. Agopyan, A.M. Nolasco, L. Pimentel, Plant fibre reinforced

ACCEPTED MANUSCRIPT

349

[13]

W. Zhu, P.J.M. Bartos, Application of depth-sensing microindentation testing to study

350

of interfacial transition zone in reinforced concrete, Cem. Concr. Res. 30 (2000) 1299–1304.

351

doi:10.1016/S0008-8846(00)00322-7.

352

[14]

353

Cement-based Composites, J. Proc. 83 (1986) 597–605.

354

[15]

355

Fiber-Reinforced Cement Paste, Mater. J. 97 (2000) 162–167.

356

[16]

357

modulus using load and displacement sensing indentation experiments, Mater. Res. Soc. 7

358

(1992) 1564–1583.

359

[17]

360

prediction of macroscale elastic properties of high performance cementitious composites,

361

Cem. Concr. Compos. 45 (2014) 57–68. doi:10.1016/j.cemconcomp.2013.09.013.

362

[18]

363

Effect of fibre morphology on flocculation of fibre-cement suspensions, Cem. Concr. Res. 39

364

(2009) 1017–1022. doi:10.1016/j.cemconres.2009.07.010.

365

[19]

366

Standard Specification for Portland Cement.

367

[20]

368

study on vegetable wastes as reinforcement in extruded fibre-cement., in: Int. Conf. Non-

369

Conventional Mater. Technol. Ecol. Mater. Technol. Sustain. Constr., 2007, Maceió. Anais do

370

Brasil-NOCMAT. (Abmtenc) Maceió., 2007.

371

[21]

372

Supercritical carbonation treatment on extruded fibre–cement reinforced with vegetable

373

fibres, Cem. Concr. Compos. 56 (2015) 84–94. doi:10.1016/j.cemconcomp.2014.11.007.

374

[22]

375

Rocco Lahr, Cellulose modified fibres in cement based composites, Compos. Part A Appl.

376

Sci. Manuf. 40 (2009) 2046–2053. doi:10.1016/j.compositesa.2009.09.016.

377

[23]

378

Pescatori Silva, H. Savastano Jr., Effect of eucalyptus pulp refining on the performance and

379

durability of fibre-cement composites., J. Trop. For. Sci. 25 (2013) 400–409.

380

[24]

381

Dissolution and Carbonation of Portlandite [Ca(OH)2] Single Crystals, Environ. Sci. Technol.

382

47 (2013) 11342–11349. doi:10.1021/es402061c.

383

[25]

S. Wei, J.A. Mandel, S. Said, Study of the Interface Strength in Steel Fiber-Reinforced

RI PT

W.M. Cross, K.H. Sabnis, L. Kjerengtroen, J.J. Kellar, Microhardness Testing of

W. Oliver, G. Pharr, An improved technique for determining hardness and elastic

M AN U

SC

W.R.L. Da Silva, J. Němeček, P. Štemberk, Methodology for nanoindentation-assisted

G.H.D. Tonoli, E. Fuente, C. Monte, H. Savastano Jr, F.A. Rocco Lahr, A. Blanco,

ASTM C 150, American Society for Testing and Materials – ASTM C150/C150M-11.

TE D

Y.J.M. Soto, G.H.D. Tonoli, R.S. Teixeira, S.F. Santos, H. Savastano Jr, Prospective

AC C

EP

S.F. Santos, R. Schmidt, A.E.F.S. Almeida, G.H.D. Tonoli, H. Savastano Jr,

G.H.D. Tonoli, U.P. Rodrigues Filho, H. Savastano Jr, J. Bras, M.N. Belgacem, F.A.

G.H.D. Tonoli, S.F. Santos, R.S. Teixeira, M.A. Pereira-Da-Silva, F.A.R. Lahr, F.H.

E. Ruiz-Agudo, K. Kudłacz, C. V. Putnis, A. Putnis, C. Rodriguez-Navarro,

J.A. Larbi, J.M.J.M. Bijen, Interaction of polymers with portland cement during

ACCEPTED MANUSCRIPT

384

hydration. A study, Cem. Concr. Res. 20 (1990) 139–147. doi:10.1016/0008-8846(90)90124-

385

G.

386

[26]

387

polymer modification on the formation of high sulphoaluminate or ettringite - type (AFt)

388

crystals in polymer-modified mortars, Cem. Concr. Res. 24 (1994) 1492–1494.

389

doi:10.1016/0008-8846(94)90163-5.

390

[27]

H.F.W. Taylor, Cement chemistry, London: Academic press limited, 1990.

391

[28]

J.I. Escalante-Garcia, G. Mendoza, J.H. Sharp, Indirect determination of the Ca/Si

392

ratio of the C-S-H gel in Portland cements, Cem. Concr. Res. 29 (1999) 1999–2003.

393

doi:10.1016/S0008-8846(99)00191-X.

394

[29]

395

cycling on pulp fiber-cement composites, Cem. Concr. Res. 36 (2006) 1240–1251.

396

doi:10.1016/j.cemconres.2006.03.020.

397

[30]

398

nanoindentation testing to study of the interfacial transition zone in steel fiber reinforced

399

mortar, Cem. Concr. Res. 39 (2009) 701–715. doi:10.1016/j.cemconres.2009.05.002.

400

[31]

401

Adv. Cem. Based Mater. 4 (1996) 48–57. doi:10.1016/1065-7355(96)00035-1.

402

[32]

403

micromechanical properties of fibre reinforced cementitious composite., in: 6th RILEM

404

Symp. Fibre Reinf. Concr., BEFIB, 2004, Varenna, Italy, (2004) pp. 401–410., 2004: pp.

405

401–410.

406

[33]

407

In-built nanotechnology ,” Cerâmica. 55 (2009) 199–205. (in portuguese).

408

[34]

409

nanoindentation of elastic modulus and hardness of pure constituents of Portland cement

410

clinker, Cem. Concr. Res. 31 (2001) 555–561. doi:10.1016/S0008-8846(00)00505-6.

411

[35]

412

cement composites cured in a normal environment, Int. J. Cem. Compos. Light. Concr. 11

413

(1989) 99–109. doi:10.1016/0262-5075(89)90120-6.

414

[36]

415

sensitive sisal and coconut fibres in cement mortar composites, Cem. Concr. Compos. 22

416

(2000) 127–143. doi:10.1016/S0958-9465(99)00039-6.

417

[37]

418

composites to wet/dry cycling, Cem. Concr. Res. 35 (2005) 1646–1649.

RI PT

M.U.K. Afridi, Z.U. Chaudhary, Y. Ohama, K. Demura, M.Z. Iqbal, Effects of

M AN U

SC

B.J. Mohr, J.J. Biernacki, K.E. Kurtis, Microstructural and chemical effects of wet/dry

X.H. Wang, S. Jacobsen, J.Y. He, Z.L. Zhang, S.F. Lee, H.L. Lein, Application of

S. Igarashi, A. Bentur, S. Mindess, Microhardness testing of cementitious materials,

TE D

J. Meček, P. Kabele, Z. Bittnar, Nanoindentation based assessment of

EP

H.L. Rossetto, M.F. de Souza, V.C. Pandolfelli, Adesão em materiais cimentícios : “

AC C

K. Velez, S. Maximilien, D. Damidot, G. Fantozzi, F. Sorrentino, Determination by

A. Bentur, S.A.S. Akers, The microstructure and ageing of cellulose fibre reinforced

R.D. Tolêdo Filho, K. Scrivener, G.L. England, K. Ghavami, Durability of alkali-

B.J. Mohr, H. Nanko, K.E. Kurtis, Durability of thermomechanical pulp fiber-cement

ACCEPTED MANUSCRIPT

419

doi:10.1016/j.cemconres.2005.04.005.

420

[38]

421

to wet/dry cycling, Cem. Concr. Compos. 27 (2005) 435–448.

422

doi:10.1016/j.cemconcomp.2004.07.006.

423

[39]

424

and durability of cement based composites reinforced with refined sisal pulp, Mater. Manuf.

425

Process. 22 (2007) 149–156. doi:10.1080/10426910601062065.

B.J. Mohr, H. Nanko, K.E. Kurtis, Durability of kraft pulp fiber – cement composites

426 427 428

SC

429 430

M AN U

431 432 433 434 435 436

441 442 443 444 445 446 447 448 449 450 451 452 453

EP

440

AC C

439

TE D

437 438

RI PT

G.H.D. Tonoli, A.P. Joaquim, M.-A. Arsène, K. Bilba, H. Savastano Jr, Performance

454

ACCEPTED MANUSCRIPT

Table

455 456 457 458 459

Table 1. Physical characteristics of the unbleached eucalyptus pulp [18]. Table 2. Mix design used in the production of the composites. Table 3. Average and standard deviation values of elastic modulus and hardness obtained for

461

each structure of the composite by nanoindentation technique1

462 463 464

SC

465 466

M AN U

467 468 469 470 471 472

477 478 479 480 481 482 483 484 485 486 487 488 489

EP

476

AC C

475

TE D

473 474

RI PT

460

490

ACCEPTED MANUSCRIPT

Figure

491 492

Figure 1 – (a) Extruder machine used for molding; (b) side view showing the mass exit

493

through the die; and (c) details of the operating mechanism of the extrusion process (adapted

494

from [16]).

495 Figure 2 – Left: Scanning electron microscopy (SEM) micrographs in back scattering electron

497

(BSE) mode of the polished cross-section of an extruded composite. Right: Energy dispersive

498

spectra (EDS) referring to the fiber-matrix interface (upper) and to the bulk matrix (bottom).

RI PT

496

499

Figure 3 – AFM topography image of the interface fracture. Arrows show the possible

501

Ca(OH)2 with carbonated production in the interfacial zone between the cellulose fiber and

502

cement matrix.

M AN U

SC

500

503 504

Figure 4 – Scanning electron microscopy (SEM) image in backscattering electron (BSE)

505

mode of the polished cross-section in an extruded composite. Energy dispersive spectra

506

(EDS) refer to the composition of the anhydrous grain (spot A) and bulk matrix region (spot

507

B).

TE D

508 509

Figure 5 – (a) Light micrograph of the nanoindentation spots applied in line along the bulk

510

section of the composite; (b) individual values of elastic modulus for each spot of the

511

micrograph; and (c) individual values of hardness for each spot of the micrograph.

EP

512

Figure 6 – (a) Light micrograph of the nanoindentation spots applied in line along the

514

different structures (anhydrous grain, bulk density, cellulose fiber and interfacial/transition

515

zone between fiber and matrix) of the composite; (b) individual values of elastic modulus for

516

each spot of the micrograph; and (c) individual values of hardness for each spot of the

517

micrograph.

518

AC C

513

519

Figure 7 – (a) Scanning electron microscopy (SEM) micrographs in back scattering electron

520

(BSE) mode of the polished cross-section of an extruded composite; and (b) energy dispersive

521

spectra (EDS) of the spots 1 and 2 in the SEM micrographs.

522 523 524

525

ACCEPTED MANUSCRIPT

Table 1 Average length (mm)

Average width (µm)

Aspect Ratio

Fibrous material (106 fibers/g)

Content of fines by mass (%)

0.83 ± 0.05

16.4 ± 0.2

51

18.17 ± 1.11

25.7 ± 0.6

526 527

RI PT

528 529 530 531

SC

532 533 534

M AN U

535 536 537 538 539

543 544 545 546 547 548 549 550 551 552 553 554 555 556

EP

542

AC C

541

TE D

540

558 559

ACCEPTED MANUSCRIPT

Table 2 Raw material

Content (% by mass)

Portland cement (CPV-ARI) a

70

Limestone filler b

27

Unbleached eucalyptus pulp c

3

(a) ASTM C150 type I [19], provided by Caue, (b) Itaú, (c) Fibria S.A.

RI PT

557

560 561 562

SC

563 564 565

M AN U

566 567 568 569 570

574 575 576 577 578 579 580 581 582 583 584 585 586 587

EP

573

AC C

572

TE D

571

ACCEPTED MANUSCRIPT

588

590 591 592

Table 3 Structures

Elastic modulus (GPa)

Hardness (GPa)

Interfacial/transition zone

17.2 ± 5.6 c

0.4 ± 0.2 c

Bulk matrix

72.7 ± 14.3 b

5.3 ± 1.8 b

Anhydrous grain

89.9 ± 17.1 b

4.5 ± 1.9 b

Cellulosic fiber

144.3 ± 48.9 a

8.9 ± 2.5 a

1

Lowercase letters (a, b and c) in the same column represent comparisons between conditions of the composites. Different letters indicate significant differences amongst the properties of the composites.

593

SC

594 595

M AN U

596 597 598 599 600

605 606 607 608 609 610 611 612 613 614 615 616 617 618

EP

604

AC C

603

TE D

601 602

RI PT

589

ACCEPTED MANUSCRIPT

SC

RI PT

619

621

M AN U

620 Figure 1

622 623 624

628 629 630 631 632 633 634 635 636 637 638 639 640 641 642

EP

627

AC C

626

TE D

625

ACCEPTED MANUSCRIPT

643

RI PT

Interface

SC

Bulk matrix

M AN U

644 645 646

Figure 2

647 648 649

653 654 655 656 657 658 659 660 661 662 663 664 665 666

EP

652

AC C

651

TE D

650

ACCEPTED MANUSCRIPT

RI PT

667

SC

5

µm 668 669 670

Figure 3

671 672

676 677 678 679 680 681 682 683 684 685 686 687 688 689

EP

675

AC C

674

TE D

673

M AN U

10

ACCEPTED MANUSCRIPT

690

Anhydrous grain

B

SC

Bulk matrix

RI PT

A

691 692 Figure 4

M AN U

693 694 695 696 697

701 702 703 704 705 706 707 708 709 710 711 712 713

EP

700

AC C

699

TE D

698

ACCEPTED MANUSCRIPT

M AN U

SC

RI PT

(a)

AC C

EP

TE D

(b)

714 715

(c) Figure 5

ACCEPTED MANUSCRIPT

Transition zone

81

Cellulosic fibre Anhydrous grain

SC

71

RI PT

101 91

Bulk matrix

(b)

AC C

EP

TE D

M AN U

(a)

M AN U

SC

RI PT

ACCEPTED MANUSCRIPT

(c) 716 717

Figure 6

718

722 723 724 725 726 727 728 729 730 731 732 733 734 735

EP

721

AC C

720

TE D

719

ACCEPTED MANUSCRIPT

736

1 Hydration products in the cellulosic fiber

1 Cellulosic fiber

SC

(a)

(b)

737 738

Anhydrous grain

M AN U

30 µm

Bulk matrix

Transition zone

RI PT

2

Figure 7

AC C

EP

TE D

739

2