Slurry erosion-corrosion resistance and microbial corrosion electrochemical characteristics of HVOF sprayed WC-10Co-4Cr coating for offshore hydraulic machinery

Slurry erosion-corrosion resistance and microbial corrosion electrochemical characteristics of HVOF sprayed WC-10Co-4Cr coating for offshore hydraulic machinery

Accepted Manuscript Slurry erosion-corrosion resistance and microbial corrosion electrochemical characteristics of HVOF sprayed WC-10Co-4Cr coating fo...

10MB Sizes 0 Downloads 22 Views

Accepted Manuscript Slurry erosion-corrosion resistance and microbial corrosion electrochemical characteristics of HVOF sprayed WC-10Co-4Cr coating for offshore hydraulic machinery

Sheng Hong, Yuping Wu, Wenwen Gao, Jianfeng Zhang, Yugui Zheng, Yuan Zheng PII: DOI: Reference:

S0263-4368(18)30026-X doi:10.1016/j.ijrmhm.2018.02.019 RMHM 4679

To appear in:

International Journal of Refractory Metals and Hard Materials

Received date: Revised date: Accepted date:

10 January 2018 5 February 2018 18 February 2018

Please cite this article as: Sheng Hong, Yuping Wu, Wenwen Gao, Jianfeng Zhang, Yugui Zheng, Yuan Zheng , Slurry erosion-corrosion resistance and microbial corrosion electrochemical characteristics of HVOF sprayed WC-10Co-4Cr coating for offshore hydraulic machinery. The address for the corresponding author was captured as affiliation for all authors. Please check if appropriate. Rmhm(2017), doi:10.1016/ j.ijrmhm.2018.02.019

This is a PDF file of an unedited manuscript that has been accepted for publication. As a service to our customers we are providing this early version of the manuscript. The manuscript will undergo copyediting, typesetting, and review of the resulting proof before it is published in its final form. Please note that during the production process errors may be discovered which could affect the content, and all legal disclaimers that apply to the journal pertain.

ACCEPTED MANUSCRIPT Slurry erosion-corrosion resistance and microbial corrosion electrochemical characteristics of HVOF sprayed WC-10Co-4Cr coating for offshore hydraulic machinery

PT

Sheng Honga,b,c*, Yuping Wua,c, Wenwen Gaoa, Jianfeng Zhanga, Yugui Zhengc, Yuan

a

SC

RI

Zhengd

College of Mechanics and Materials, Hohai University, 8 Focheng West Road,

Material Corrosion and Protection Key Laboratory of Sichuan Province, 180

MA

b

NU

Nanjing 211100, PR China

Xueyuan Street, Zigong 643000, PR China Key Laboratory of Nuclear Materials and Safety Assessment, Institute of Metal

D

c

China

National Engineering Research Center of Water Resources Efficient Utilization and

CE

d

PT E

Research, Chinese Academy of Sciences, 62 Wencui Road, Shenyang 110016, PR

AC

Engineering Safety, Hohai University, 1 Xikang Road, Nanjing 210098, PR China



Corresponding author: Tel:+86-25-83787233; fax: +86-25-83787233

E-mail address: [email protected] (S. Hong), [email protected] (Y.P. Wu). 1

ACCEPTED MANUSCRIPT Abstract

The slurry erosion-corrosion and microbial corrosion electrochemical behavior of high-velocity oxygen-fuel (HVOF) sprayed WC-10Co-4Cr cermet coatings and the stainless

steel

1Cr18Ni9Ti

were

both

investigated.

The

slurry

PT

reference

RI

erosion-corrosion test was performed in a rotating disk rig facility with circulating

SC

system using distilled water and 3.5 wt.% NaCl slurries. The microbial influenced corrosion behavior in the presence of SRB was evaluated by electrochemical

NU

measurement. The results showed that WC-10Co-4Cr coating exhibited higher slurry

MA

erosion-corrosion resistance compared to the stainless steel 1Cr18Ni9Ti in both distilled water and 3.5 wt.% NaCl slurries. The evolution of the slurry erosion

D

mechanism of the coatings with the augment of NaCl concentration was cracks and

PT E

microchipping in distilled water slurry, and a combination of detachment of binder phase, microchipping and fragments in 3.5 wt.% NaCl slurry. Potentiodynamic

CE

polarization and electrochemical impendence spectroscopy (EIS) results showed that

AC

the WC-10Co-4Cr coating had a comparable microbial influenced corrosion resistance in seawater with SRB as compared to the stainless steel 1Cr18Ni9Ti.

Keywords: High-velocity oxygen-fuel; Slurry erosion; Microbial influenced corrosion; Sulfate-reducing bacteria; WC-10Co-4Cr.

2

ACCEPTED MANUSCRIPT 1. Introduction Many flow-handling components of hydraulic power plants situated in the coastal region are exposed to an environment that contains sand particles and microorganisms. When the flow-handling part of offshore hydraulic machinery works, it always

PT

follows the high-velocity impact of liquid-solid streams result in slurry erosion failure.

RI

However, microbial corrosion displays a strong tendency to accelerate material

SC

deterioration of infrastructure when the machine stops [1,2]. Both slurry erosion and microbial corrosion cause reductions in the efficient operation of hydraulic machinery

NU

and substantial economic losses in offshore hydraulic power plants. This urgent

MA

problem is generally solved through hydrodynamics optimization, mechanical construction design and material exploitation [3-5]. In particular, WC-Co hardmetals

D

are preferred material choice for reductions of sliding wear, abrasion, tribo-corrosion

PT E

and slurry erosion damage due to the combination of high hardness and adequate fracture toughness [6,7]. Besides hardness and toughness, WC grain size and binder

CE

mean free path also affect the erosion resistance of WC-Co hardmetals [8-10].

AC

Due to the prevalence of surface treatment techniques in industrial applications, great attentions of the researchers worldwide have been paid to the use of thermal sprayed coatings to improve the slurry erosion and microbial corrosion resistance of steel components for prolonging the service life of offshore hydraulic machinery [11-13]. Among all thermal sprayed coatings, the WC-Co system cermet coatings are often considered to be the protection of the metallic components in high wear, erosion and corrosion-resistant applications. Various spraying techniques, such as detonation 3

ACCEPTED MANUSCRIPT spraying [14,15], plasma spraying [16-18], and high-velocity oxygen-fuel (HVOF) spraying [19-23] have been employed to fabricate the WC-Co system cermet material. Compared with other thermal spraying methods, HVOF spraying is capable of producing a dense WC-Co system cermet coating with low porosity, limited oxide

PT

content, less decarburization, high hardness and superior bond strength [24]. It is

RI

evident from literature that slurry erosion resistance of HVOF sprayed WC-Co system

SC

cermet coating was related not only to impingement velocity and impact angle, solid concentration, size and shape of erodent, but also to carbide grain size, binder matrix

NU

property, porosity and hardness of the coatings [19,25,26]. The literature survey

MA

described above demonstrated that most investigations on the slurry erosion behavior of the coatings were used the jet impingement method. However, the application of

D

the rotating disc arrangements method in studying the slurry erosion-corrosion

PT E

behavior of HVOF sprayed WC-Co system cermet coatings is still limited, with which a rotation condition of actual hydraulic pump impellers can be simulated. Furthermore,

CE

it has also been observed that, there are not much studies available in the literature

AC

related to the microbial influenced corrosion behavior of HVOF sprayed WC-Co based coatings except studies on their corrosion properties under other corrosive environments, such as artificial seawater electrolyte, 3.5 wt.% NaCl solution and acidic solution [27-29]. In particular, sulfate-reducing bacteria (SRB)-influenced corrosion as a predominant form of microbial influenced corrosion involved the iron-derived electron transfer pathway, the consumption of cathodic hydrogen, and the chemical attack by sulfate, sulfite, thiosulfate, hydrogen sulfide and other acidic 4

ACCEPTED MANUSCRIPT organisms [30,31]. In a previous work, the present authors obtained the optimal spray parameter of HVOF sprayed conventional WC-10Co-4Cr coatings by investigating the correlation between the spray parameters and the porosity. The coating obtained by the optimum

PT

spraying condition exhibited better corrosion resistance and seemed to be an

RI

alternative to hard chromium coating in 3.5 wt.% NaCl solution [32]. This work is an

SC

extension of the reported research. In the current study, the slurry erosion-corrosion performance and the microbial influenced corrosion behavior in the presence of SRB

NU

of the WC-10Co-4Cr coating and the reference stainless steel 1Cr18Ni9Ti were both

MA

investigated using rotating disc arrangements method and electrochemical methods (e.g., potentiodynamic polarization and electrochemical impendence spectroscopy

PT E

D

(EIS)), respectively.

2. Experimental procedure

CE

2.1 Sample preparation

AC

Feedstock material used in this study was a commercial agglomerated and sintered WC-10 wt.% Co-4 wt.% Cr powder (Large Solar Thermal Spraying Material Co. Ltd, Chengdu, China). The powders were deposited onto 1Cr18Ni9Ti stainless steel substrates using a commercial HVOF spray system (Praxair Tafa-JP8000, USA). Prior to the HVOF spraying, the substrate samples were pre-cleaned in acetone, dried in hot air, and then grit blasted with 30 mesh Al2O3 to enhance the bond strength of as-sprayed coating to substrate by increasing the surface roughness. The HVOF 5

ACCEPTED MANUSCRIPT spraying of the powders was carried out at a kerosene flow rate of 0.38 L·min-1, an oxygen flow rate of 897 L·min-1, a spray distance of 300 mm, an argon carrier gas flow rate of 10.86 L·min-1, a powder feed rate of 5 rpm, and a spray gun speed of 280 mm·s-1. The thickness of the as-sprayed coatings was about 400 μm, which was

PT

controlled by the number of passes of the spray gun. Then the coating specimens were

RI

wire cut, ground and polished for slurry erosion and microbial corrosion testing.

SC

Stainless steel 1Cr18Ni9Ti was also tested in the same condition for comparison based on its wide applications in offshore hydraulic machinery. Details of the

NU

microstructures, thermostability and formation mechanisms of the HVOF sprayed

MA

WC-10Co-4Cr coating has been reported in the literature [33].

D

2.2 Slurry erosion test

PT E

The slurry erosion experiments were carried out using a rotating disk rig facility with circulating system. Details of the slurry erosion test apparatus and its specimen's

CE

dimension were described in our previous research [34]. Prior to the test, specimens

AC

with an average surface roughness Ra=0.02 μm were cleaned with acetone in an ultrasonic bath, dried in hot air, and weighed by an electronic balance. Then, specimens were fixed on the disk that controlled by a motor. In the testing process, the slurry solution consisted of water and commercial silica sand with the grain size of 70~150 mesh. The slurry solution containing 3.5 wt.% NaCl and silica sand was also used for comparison. The sand concentration and the rotation speed of specimen were 10 kg·m-3 and 18 m·s-1, respectively. The slurry erosion test time was set to a constant 6

ACCEPTED MANUSCRIPT value of 10 h. After each slurry erosion test, specimens were degreased, rinsed, dried and weighed periodically by an analytical balance with an accuracy of 0.1 mg to determine mass loss. The surface morphologies of specimens after slurry erosion were observed by a scanning electron microscope (SEM, Hitachi S-3400N, Japan) with an

SC

RI

to make sure a good repeatability of the experiment result.

PT

energy dispersive spectroscopy (EDS, EX250). Each test was repeated at least thrice

2.3 Microbial corrosion electrochemical measurement

NU

The SRB used in this study were obtained from muddy sediment in Jiaozhou Bay of

MA

Qingdao. Fresh marine sediment was added into a sterile modified Postgate’s C (PGC) medium to enrich anaerobic bacteria. The bacteria were subsequently purified in

D

sterile agar plates by picking up several single colonies with a sterile inoculation loop.

PT E

The procedure was repeated until the colonies of single SRB strain were formed on the solid PGC medium. The modified Postgate’s C culture solution contained 0.5 g

CE

KH2PO4, 1.0 g NH4Cl, 0.06 g CaCl2·6H2O, 0.06 g MgSO4·7H2O, 6 mL 70 % sodium

AC

lactate, 1.0 g yeast extract, and 0.3 g sodium citrate in 1 L seawater from Qingdao offshore area. The pH value was adjusted to 7.0 using the appropriate amount of sodium hydroxide before the medium was autoclaved at 121 °C for 20 min. All the electrochemical tests were performed at 30 °C using the Solartron SI1287 electrochemical interface and SI1260 impedance/gain phase analyzer control systems. Before tests, working electrode, counter electrode, rubber stoppers and salt bridge were degreased with ethanol using an ultrasonic bath followed by exposure to a UV 7

ACCEPTED MANUSCRIPT lamp for 20 min. The electrodes used in the present study were as follows: a working electrode; a ruthenium-titanium counter electrode; and a silver/silver chloride (Ag/AgCl, 3M KCl) reference electrode (CH Instruments, Inc.). The EIS data were measured at open circuit potential (OCP) by applying a sinusoidal potential excitation

PT

of 10 mV amplitude in a frequency range of 100 kHz~10 mHz. The experimental data

RI

were interpreted on the basis of equivalent circuits using the software ZsimpWin3.21

SC

to obtain the fitting parameters. The potentiodynamic polarization curves were measured with a fixed sweep rate of 0.5 mV·s-1. The corrosion current density (icorr)

NU

and corrosion potential (Ecorr) were obtained as the intersection point of linear fits to

MA

the anodic and cathodic polarization curves, according to the Tafel extrapolation

PT E

3. Results and discussion

D

technique.

3.1 Slurry erosion-corrosion performance of nanostructured WC-CoCr coatings

CE

Fig. 1 shows the effects of chloride ions concentration on mass loss rate of HVOF

AC

sprayed WC-10Co-4Cr coating and stainless steel 1Cr18Ni9Ti. As can be seen, the erosion rate increases as the slurry erosion-corrosion condition becomes more severe, which is in accord with the results observed in previous investigation of HVOF sprayed Fe-based amorphous metallic coatings [34]. This is because that both uniform corrosion and pitting corrosion are more pronounced under the combined action of slurry erosion and corrosion [35]. After eroded for 10 h, the mass loss rates of the WC-10Co-4Cr coating in distilled water slurry and 3.5 wt.% NaCl slurry are 8

ACCEPTED MANUSCRIPT 0.19±0.02 and 0.29±0.04 mg·cm-2·h-1, respectively, whereas the mass loss rates of the stainless steel 1Cr18Ni9Ti in distilled water slurry and 3.5 wt.% NaCl slurry are 1.43±0.09 and 2.37±0.11 mg·cm-2·h-1, respectively. This indicates that the WC-10Co-4Cr coating exhibits a superior slurry erosion-corrosion resistance

PT

compared to the stainless steel 1Cr18Ni9Ti and the difference between the coating

RI

and the stainless steel is enhanced with the augment of NaCl concentration. Firstly,

SC

this could be explained that the hardness of the WC-10Co-4Cr coating (1423 Hv0.1) is about 7 times higher than that of the stainless steel 1Cr18Ni9Ti (203 Hv0.1) since the

NU

hardness has a great influence on the slurry erosion resistance [36]. Secondly, the low

MA

dissolution rate of W oxides in the passive film of the WC-10Co-4Cr coating would suppress passive dissolution and inhibit slurry erosion-corrosion damage, although the

D

stability of passive film and the ability of repassivation for the WC-10Co-4Cr coating

PT E

and the stainless steel 1Cr18Ni9Ti are both reduced in severe erosive conditions [35,37]. Moreover, high elastic modulus and fracture toughness of the WC-10Co-4Cr

CE

coating are vital to enhance the wear and slurry erosion resistance, which has been

AC

indicated by other researchers [12,38]. SEM and EDS were taken to gain further information about the slurry erosion-corrosion mechanisms in different slurry solutions from eroded surfaces of the WC-10Co-4Cr coating and the stainless steel 1Cr18Ni9Ti. Figs. 2 and 3 show the SEM images of the WC-10Co-4Cr coating and the stainless steel 1Cr18Ni9Ti after slurry erosion-corrosion tests for 10 h in distilled water and 3.5 wt.% NaCl slurries, respectively. It can be seen clearly that the WC-10Co-4Cr coating (Figs. 2(a) and 3(a)) 9

ACCEPTED MANUSCRIPT has relatively smoother eroded surfaces as compared to the stainless steel 1Cr18Ni9Ti (Figs. 2(c) and 3(c)) in both slurries. This is consistent with the mass loss rate results. As shown in Fig. 2(b), cracks and microchipping are detected on the surface of the coating after eroded in distilled water slurry for 10 h, confirming that the mass loss

PT

begins around the peripheries of micropores, propagates into the binder phase, and

RI

follows by a fatigue process. This phenomenon is in good agreement with the results

SC

reported by other researchers [14,39]. Fig. 2(d) shows formation of ploughing and signs of lips, microcutting and plastic deformation in the stainless steel after eroded

NU

for 10 h, which are responsible for the material removal. In case of 3.5 wt.% NaCl

MA

slurry testing, detachment of binder phase resulted from the micro-galvanic cells between the WC phase and the CoCr binder is observed in Fig. 3(b), which lead to

D

formation of more number of microchipping and fragments on the coating surface.

PT E

Under same condition, corrosion pits are seen for the stainless steel, which is verified by the EDS analysis. The chemical composition of point A in Fig. 3(d) is Fe 52.38 -

CE

Cr 14.80 - Ni 6.51 - C 17.43 - O 7.88 - C 17.43 (at.%), indicating that some iron

AC

oxides are formed as a result of simultaneous action of localized corrosion and repetitive impingements.

3.2 Microbial corrosion electrochemical behavior in the presence of SRB EIS is a suitable technique to characterize the electrochemical processes in microbial influenced corrosion, including the reactions at the metal/solution interface and the formation of natural oxidation films, SRB biofilms and corrosive products [40]. Fig. 4 10

ACCEPTED MANUSCRIPT shows the Time-dependent Nyquist plots and the corresponding Bode plots of HVOF sprayed WC-10Co-4Cr coating and stainless steel 1Cr18Ni9Ti exposed to the seawater with SRB. As shown in Fig. 4(a), the diameter of Nyquist plots increases over time for the WC-10Co-4Cr coating. However, an increase in the diameter from 3

PT

h to 8 d is observed for the stainless steel 1Cr18Ni9Ti, and the diameter decreases

RI

after 8 d of exposure to the seawater with SRB (Fig. 4(c)). The diameters of Nyquist

SC

plots for the stainless steel are always larger than those for the coating, indicating that the stainless steel 1Cr18Ni9Ti has a slower corrosion rate compared to the

NU

WC-10Co-4Cr coating. Different from the cases of the coatings where two maxima

MA

are observed at the Bode phase angle plots during the immersion period (Fig. 4(b)), only one time constant is observed for the stainless steel 1Cr18Ni9Ti from 3 h to 2 d,

D

and a broad time constant joined by two time constants appears after 5 d (Fig. 4(d)).

PT E

The conjunction of the two time constants may be attributed to the similar frequency responses of the oxidation of metal surface and the formation of electric double layer

CE

[31]. For a better explanation to microbial influenced corrosion behavior, equivalent

AC

circuits are used to simulate the experimental impedance diagrams by ZSimpWin commercial software (USA). The chi square (χ2) value reaches the level of 10-3, which ensures the quality of fitting. The equivalent circuits describing the electrochemical reactions for the WC-10Co-4Cr coating and the stainless steel 1Cr18Ni9Ti in seawater with SRB are shown in Fig. 5. According to the characteristic of Nyquist plots of the coating after immersion for 3 h to 15 d and the stainless steel after immersion for 5 d, the equivalent circuits 11

ACCEPTED MANUSCRIPT with two time constants are used to fit the EIS data. The constant phase element (CPE or Q) is interpreted by dispersion effects from surface roughness and heterogeneous biofilm of the sample [41], which can be described as ZQ=Y0-1(jω)-n (0
PT

Fig. 5(b) consisting of an additional element Warburg impedance (Zw) is used to fit

RI

the Nyquist plots of the coating after immersion for 2 d, where the parameter reflects

SC

the diffusion coefficient, the characteristic of stagnant layer, and the mass-transfer reaction based on the accumulation of corrosive products in pores [42]. According to

NU

Ahn et al. [43] and Liu et al. [44], the Warburg impedance is usually employed to

MA

represent semi-infinite diffusion process, which suggests a diffusion controlled mechanism in electrochemical systems. Fig. 5(c) shows an equivalent circuit based on

D

a single layer which can be satisfactorily used for fitting the Nyquist plots of the

PT E

stainless steel after immersion for 3 h to 2 d. In the case of the WC-10Co-4Cr coating, Rs, Rp, Rct, Qc, and Qdl represent the resistance of electrolyte solution, the resistance of

CE

pores, the resistance of charge transfer, the capacitance of the coating, and the

AC

capacitance of the double layer, respectively. Besides, Rf and Qf correspond to the resistance and the capacitance of surface film for the stainless steel 1Cr18Ni9Ti, respectively.

In this study, the fitting values of Rct shown in Fig. 6 are important parameter for the evaluation of corrosion rate, since the values of Rct are more than thousand times higher than those of Rs, Rp and/or Rf. For the plots of the WC-10Co-4Cr coating recorded at the initial stage, the Rct value decreases from 234 k·cm2 at 3 h to 92 12

ACCEPTED MANUSCRIPT k·cm2 at 5 d. This is associated with the penetration of the corrosion medium to the interior of the coating and the dissolution of the active zones inside the coating, although pores and microcracks are limited. The increase in Rct value from 92 k·cm2 at 5 d to 196 k·cm2 at 8 d is attributed to the plugging of the electron transfer

PT

pathway that influenced by the accumulation of corrosive products and the formation

RI

of SRB biofilms on the coating surface [45]. After the increase, Rct value decreases

SC

slightly during the late period, indicating that the corrosion of oxide films and the surface inhomogeneity are both increasing due to continuous microbial influenced

NU

corrosion. The characteristic in Rct shift for the stainless steel 1Cr18Ni9Ti is opposite

MA

to that of the coating at the initial stage, and the variation of the Rct value is much larger. This could be explained that the natural oxidizing Cr2O3 formed on the

D

stainless steel sample is a dense passive film, which will hamper the transportation of

PT E

corrosive ions and inhibits the corrosion process [46]. As the immersion time prolongs, the Rct value decreases from 1063 k·cm2 at 5 d to 665 k·cm2 at 15 d. The

CE

reason may be that the natural oxidizing film breaks and the chemical or

AC

electrochemical reactions are influenced by SRB metabolic activity. When the sulfide deposits on the surface, the cathodic polarization process within the crevice resulted from the partial destruction of oxidizing film will be facilitated, which increases the electron transfer rate [47]. Furthermore, it can be seen that the Rct values of the WC-10Co-4Cr coating are lower than those of the stainless steel 1Cr18Ni9Ti at the corresponding time points, suggesting that the corrosion resistance of the coating is lower than the stainless steel in seawater with SRB. 13

ACCEPTED MANUSCRIPT Figs. 7(a) and (b) show the potentiodynamic polarization curves of HVOF sprayed WC-10Co-4Cr coating and stainless steel 1Cr18Ni9Ti exposed to the seawater with SRB for different time, respectively. It can be obviously seen that polarization curve behaviors of the coating and the stainless steel are both influenced

PT

by the adhesion of SRB biofilms. Table 1 exhibits the values of the electrochemical

RI

corrosion parameters extracted from the curves, such as corrosion potential (Ecorr) and

SC

corrosion current density (icorr). As shown in Table 1, the effect of SRB on the corrosion is quite different for the coating and the stainless steel at the initial stage.

NU

The presence of bacteria triggers increases in icorr values of the coating at the first 5 d,

MA

while the stainless steel exhibits the opposite tendency. This suggests that the combined effects of corrosive ions and SRB metabolites can inhibit the formation of

D

the passive film and accelerate the corrosion process of the coating. However, the

PT E

presence of natural oxidizing film on the stainless steel surface effectively prevents microbial adhesion and inhibits biofilm growth for a while. The icorr value of the

CE

coating first decreases and then increases from 5 d to 15 d. This can be attributed to

AC

the presence of corrosive products and SRB biofilms on the coating surface, and the corrosion of oxide films accelerated by the corrosive metabolites, respectively. For the stainless steel, the increase of the icorr value from 5 d to 15 d can be explained by the partial breakage of oxidizing film and dissolution of metal under the effect of SRB metabolic activity [47]. The results of the potentiodynamic polarization curves are consistent with the EIS tests as shown in Figs. 4 and 6. In addition, the icorr values have the same order of magnitudes for the coating and the stainless steel, indicating 14

ACCEPTED MANUSCRIPT that the coating with compact and uniform structure can provide effective protection for the steel substrate in seawater with SRB. As discussed above, HVOF sprayed WC-10Co-4Cr coating exhibits a higher slurry erosion-corrosion resistance and a comparable microbial influenced corrosion resistance as compared to the stainless

PT

steel 1Cr18Ni9Ti, which provides a potentially competitive approach for offshore

SC

RI

hydraulic machinery.

4. Conclusions

NU

In this study, the WC-10Co-4Cr cermet coating was deposited on the stainless steel

MA

1Cr18Ni9Ti by HVOF spraying system. WC-10Co-4Cr coating exhibited a superior slurry erosion-corrosion resistance compared to the stainless steel 1Cr18Ni9Ti in both

D

distilled water and 3.5 wt.% NaCl slurries, and the difference between the coating and

PT E

the stainless steel was enhanced with the augment of NaCl concentration. Cracks and microchipping contributed to the slurry erosion mechanism of the coating in distilled

CE

water slurry, while the main failure mechanism of the coating was detachment of

AC

binder phase, microchipping and fragments in 3.5 wt.% NaCl slurry. Compared with stainless steel 1Cr18Ni9Ti, the WC-10Co-4Cr coating had a comparable microbial influenced corrosion resistance in seawater with SRB indicated by potentiodynamic polarization and EIS results. This study provides a potentially competitive cermet coating for use in engineering applications of offshore hydraulic machinery.

15

ACCEPTED MANUSCRIPT Acknowledgments The research was supported by the National Natural Science Foundation of China (Grant Nos. 51609067, 51579087 and 51339005), the Natural Science Foundation of Jiangsu Province of China (Grant No. BK20150806), the China Postdoctoral Science

PT

Foundation (Grant No. 2016M590404), the Opening Project of Material Corrosion

RI

and Protection Key Laboratory of Sichuan Province (Grant No. 2016CL08), and the

SC

Opening Project of CAS Key Laboratory of Nuclear Materials and Safety Assessment (Grant No. 2016NMSAKF03). Professor Jizhou Duan of Institute of Oceanology, Academy

of

Sciences

was

also

NU

Chinese

acknowledged

for

providing

AC

CE

PT E

D

MA

microbiologically induced corrosion equipment.

16

ACCEPTED MANUSCRIPT References [1] D.K. Goyal, H. Singh, H. Kumar, V. Sahni, Slurry erosion behavior of HVOF sprayed WC-10Co-4Cr and Al2O3+13TiO2 coatings on a turbine steel, Wear 289 (2012) 46-57.

PT

[2] J. Landoulsi, K. El Kirat, C. Richard, D. Feron, S. Pulvin, Enzymatic approach in

RI

microbial-influenced corrosion: A review based on stainless steels in natural

SC

waters, Environ. Sci. Technol. 42 (2008) 2233-2242.

[3] S.M. Ghaneeizad, J.F. Atkinson, S.J. Bennett, Effect of flow confinement on the

NU

hydrodynamics of circular impinging jets: implications for erosion assessment,

MA

Environ. Fluid Mech. 15 (2015) 1-25.

[4] W.R. Trenouth, B. Gharabaghi, Event-based design tool for construction site

D

erosion and sediment controls, J. Hydrol. 528 (2015) 790-795.

PT E

[5] A. Krishnamurthy, V. Gadhamshetty, R. Mukherjee, Z. Chen, W. Ren, H.M. Cheng, N. Koratkar, Passivation of microbial corrosion using a graphene coating,

CE

Carbon 56 (2013) 45-49.

AC

[6] A.J. Gant, M.G. Gee, D.D. Gohil, H.G. Jones, L.P. Orkney, Use of FIB/SEM to assess the tribo-corrosion of WC/Co hardmetals in model single point abrasion experiments, Tribol. Int. 68 (2013) 56-66. [7] A.J. Gant, J.W. Nunn, M.G. Gee, D. Gorman, D.D. Gohil, L.P. Orkney, New perspectives in hardmetal abrasion simulation, Wear 376-377 (2017) 2-14. [8] B. Roebuck, Extrapolating hardness-structure property maps in WC/Co hardmetals, Int. J. Refract. Met. Hard Mater. 24 (2006) 101-108. 17

ACCEPTED MANUSCRIPT [9] A.J. Gant, M.G. Gee, Structure-property relationships in liquid jet erosion of tungsten carbide hardmetals, Int. J. Refract. Met. Hard Mater. 27 (2009) 332-343. [10] A.J. Gant, M.G. Gee, Wear modes in slurry jet erosion of tungsten carbide

PT

hardmetals: Their relationship with microstructure and mechanical properties, Int.

RI

J. Refract. Met. Hard Mater. 49 (2015) 192-202.

SC

[11] A.S. Praveen, J. Sarangan, S. Suresh, B.H. Channabasappa, Optimization and

Ceram. Int. 42 (2016) 1094-1104.

NU

erosion wear response of NiCrSiB/WC-Co HVOF coating using Taguchi method,

MA

[12] L. Thakur, N. Arora, A study of processing and slurry erosion behaviour of multi-walled carbon nanotubes modified HVOF sprayed nano-WC-10Co-4Cr

D

coating, Surf. Coat. Technol. 309 (2017) 860-871.

PT E

[13] S. Hong, Y.P. Wu, W.W. Gao, J.F. Zhang, Y.J. Qin, Corrosion behavior of arc-sprayed Zn-Al coating in the presence of sulfate-reducing bacteria in

CE

seawater, J. Mater. Eng. Perform. 24 (2015) 4449-4455.

AC

[14] S. Bhandari, H. Singh, H. Kumar, V. Rastogi, Slurry erosion performance study of detonation gun-sprayed WC-10Co-4Cr coatings on CF8M steel under hydro-accelerated conditions, J. Therm. Spray Technol. 21 (2012) 1054-1064. [15] V. Ulianitsky, I. Batraev, D. Dudina, I. Smurov, Enhancing the properties of WC/Co detonation coatings using two-component fuels, Surf. Coat. Technol. 318 (2017) 244-249. [16] G. Di Girolamo, L. Pilloni, G. Pulci, F. Marra, Tribological characterization of 18

ACCEPTED MANUSCRIPT WC-Co plasma sprayed coatings, J. Am. Ceram. Soc. 92 (2009) 1118-1124. [17] G. Di Girolamo, F. Marra, G. Pulci, J. Tirillo, T. Valente, L. Pilloni, Microstructure and wear behavior of plasma-sprayed nanostructured WC-Co coatings, Int. J. Appl. Ceram. Technol. 10 (2013) 60-71.

PT

[18] L.J. Guo, J. Peng, G. Kou, G.G. Shi, K.Y. Dong, Oxyacetylene torch ablation

RI

resistance of Co-modified WC coating deposited on C/C composites by

SC

supersonic atmosphere plasma spraying, Ceram. Int. 43 (2017) 8989-8998. [19] L. Thakur, N. Arora, A comparative study on slurry and dry erosion behavior of

NU

HVOF sprayed WC-CoCr coatings, Wear 303 (2013) 405-411.

MA

[20] D.F. Wang, B.P. Zhang, C.C. Jia, F. Gao, Y.G. Yu, K. Chu, M.N. Zhang, X.L. Zhao, Influence of carbide grain size and crystal characteristics on the

D

microstructure and mechanical properties of HVOF-sprayed WC-CoCr coatings,

PT E

Int. J. Refract. Met. Hard Mater. 69 (2017) 138-152. [21] H.B. Wang, X.Y. Song, X.Z. Wang, X.M. Liu, X.L. Wang, Fabrication of

CE

nanostructured WC-Co coating with low decarburization, Int. J. Refract. Met.

AC

Hard Mater. 53 (2015) 92-97. [22] S. Hong, Y.P. Wu, B. Wang, J.F. Zhang, Y. Zheng, L. Qiao, The effect of temperature on the dry sliding wear behavior of HVOF sprayed nanostructured WC-CoCr coatings, Ceram. Int. 43 (2017) 458-462. [23] P.B. Mi, T. Wang, F.X. Ye, Influences of the compositions and mechanical properties of HVOF sprayed bimodal WC-Co coating on its high temperature wear performance, Int. J. Refract. Met. Hard Mater. 69 (2017) 158-163. 19

ACCEPTED MANUSCRIPT [24] S. Hong, Y.P. Wu, J.F. Zhang, Y.G. Zheng, Y. Zheng, J.R. Lin, Synergistic effect of ultrasonic cavitation erosion and corrosion of WC-CoCr and FeCrSiBMn coatings prepared by HVOF spraying, Ultrason. Sonochem. 31 (2016) 563-569.

PT

[25] R.J.K. Wood, Tribology of thermal sprayed WC-Co coatings, Int. J. Refract. Met.

RI

Hard Mater. 28 (2010) 82-94.

SC

[26] R.K. Kumar, M. Kamaraj, S. Seetharamu, S.A. Kumar, A pragmatic approach and quantitative assessment of silt erosion characteristics of HVOF and HVAF

MA

Mater. Des. 132 (2017) 79-95.

NU

processed WC-CoCr coatings and 16Cr5Ni steel for hydro turbine applications,

[27] S. Brioua, K. Belmokre, V. Debout, P. Jacquot, E. Conforto, S. Touzain, J. Creus,

D

Corrosion behavior in artificial seawater of thermal-sprayed WC-CoCr coatings

PT E

on mild steel by electrochemical impedance spectroscopy, J. Solid State Electrochem. 16 (2012) 633-648.

CE

[28] S. Hong, Y.P. Wu, Y.G. Zheng, B. Wang, W.W. Gao, J.R. Lin, Microstructure

AC

and electrochemical properties of nanostructured WC-10Co-4Cr coating prepared by HVOF spraying, Surf. Coat. Technol. 235 (2013) 582-588. [29] G. Bolelli, R. Giovanardi, L. Lusvarghi, T. Manfredini, Corrosion resistance of HVOF-sprayed coatings for hard chrome replacement, Corros. Sci. 48 (2006) 3375-3397. [30] H. Venzlaff, D. Enning, J. Srinivasan, K.J.J. Mayrhofer, A.W. Hassel, F. Widdel, M. Stratmann, Accelerated cathodic reaction in microbial corrosion of iron due 20

ACCEPTED MANUSCRIPT to direct electron uptake by sulfate-reducing bacteria, Corros. Sci. 66 (2013) 88-96. [31] F. Guan, X.F. Zhai, J.Z. Duan, J. Zhang, K. Li, B.R. Hou, Influence of sulfate-reducing bacteria on the corrosion behavior of 5052 aluminum alloy, Surf.

PT

Coat. Technol. 316 (2017) 171-179.

RI

[32] S. Hong, Y.P. Wu, Y.G. Zheng, B. Wang, W.W. Gao, G.Y. Li, G.B. Ying, J.R.

SC

Lin, Effect of spray parameters on the corrosion behavior of HVOF sprayed WC-Co-Cr coatings, J. Mater. Eng. Perform. 23(4) (2014) 1434-1439.

NU

[33] S. Hong, Y.P. Wu, W.W. Gao, B. Wang, W.M. Guo, J.R. Lin, Microstructural

MA

characterisation and microhardness distribution of HVOF sprayed WC-10Co-4Cr coating, Surf. Eng. 30(1) (2014) 53-58.

D

[34] Y. Wang, Y.G. Zheng, W. Ke, W.H. Sun, W.L. Hou, X.C. Chang, J.Q. Wang,

PT E

Slurry erosion-corrosion behaviour of high-velocity oxy-fuel (HVOF) sprayed Fe-based amorphous metallic coatings for marine pump in sand-containing NaCl

CE

solutions, Corros. Sci. 53 (2011) 3177-3185.

AC

[35] V.A. de Souza, A. Neville, Corrosion and erosion damage mechanisms during erosion-corrosion of WC-Co-Cr cermet coatings, Wear 255 (2003) 146-156. [36] A. Neville, T. Hodgkiess, J.T. Dallas, A study of the erosion-corrosion behaviour of engineering steels for marine pumping applications, Wear 186 (1995) 497-507. [37] A.C. Lloyd, J.J. Noël, S. McIntyre, D.W. Shoesmith, Cr, Mo and W alloying additions in Ni and their effect on passivity, Electrochim. Acta 49 (2004) 21

ACCEPTED MANUSCRIPT 3015-3027. [38] S. Hong, Y.P. Wu, B. Wang, J.F. Zhang, Y. Zheng, L. Qiao, Nanomechanical properties and dry sliding wear behavior of conventional and nanostructured WC-CoCr coatings prepared by HVOF spraying, Dig. J. Nanomater. Bios. 11(4)

PT

(2016) 1135-1143.

RI

[39] D.W. Wheeler, R.J.K. Wood, Erosion of hard surface coatings for use in offshore

SC

gate valves, Wear 258 (2005) 526-536.

[40] D.A. Miranda, S.A. Jaimes, J.M. Bastidas, Assessment of carbon steel

NU

microbiologically induced corrosion by electrical impedance spectroscopy, J.

MA

Solid State Electrochem. 18 (2014) 389-398.

[41] K.F. Khaled, M.N.H. Hamed, K.M. Abdel-Azim, N.S. Abdelshafi, Inhibition of

D

copper corrosion in 3.5% NaCl solutions by a new pyrimidine derivative:

PT E

electrochemical and computer simulation techniques, J. Solid State Electrochem. 15 (2011) 663-673.

CE

[42] M.M. Verdian, K. Raeissi, M. Salehi, Corrosion performance of HVOF and APS

AC

thermally sprayed NiTi intermetallic coatings in 3.5% NaCl solution, Corros. Sci. 52 (2010) 1052-1059. [43] S.H. Ahn, Y.S. Choi, J.G. Kim, J.G. Han, A study on corrosion resistance characteristics of PVD Cr-N coated steels by electrochemical method, Surf. Coat. Technol. 150 (2002) 319-326. [44] C. Liu, Q. Bi, A. Leyland, A. Matthews, An electrochemical impedance spectroscopy study of the corrosion behaviour of PVD coated steels in 0.5 N 22

ACCEPTED MANUSCRIPT NaCl aqueous solution: Part I. Establishment of equivalent circuits for EIS data modelling, Corros. Sci. 45 (2003) 1243-1256. [45] X.D. Zhao, J.Z. Duan, B.R. Hou, S.R. Wu, Effect of sulfate-reducing bacteria on corrosion behavior of mild steel in sea mud, J. Mater. Sci. Technol. 23 (2007)

PT

323-328.

RI

[46] G. Gunasekaran, S. Chongdar, S.N. Gaonkar, P. Kumar, Influence of bacteria on

SC

film formation inhibiting corrosion, Corros. Sci. 46 (2004) 1953-1967. [47] X. Chen, G.F. Wang, F.J. Gao, Y.L. Wang, C. He, Effects of sulphate-reducing

NU

bacteria on crevice corrosion in X70 pipeline steel under disbonded coatings,

AC

CE

PT E

D

MA

Corros. Sci. 101 (2015) 1-11.

23

ACCEPTED MANUSCRIPT Figure captions:

Fig. 1 Mass loss rates of HVOF sprayed WC-10Co-4Cr coating and stainless steel 1Cr18Ni9Ti at 18 m·s-1 in distilled water and 3.5 wt.% NaCl slurries (sand content:

PT

10 kg·m-3, sand size: 75~150 mesh)

RI

Fig. 2 SEM images of HVOF sprayed WC-10Co-4Cr coating (a,b) and stainless steel

content: 10 kg·m-3, sand size: 75~150 mesh)

SC

1Cr18Ni9Ti (c,d) after eroded for 10 h at 18 m·s-1 in distilled water slurry (sand

NU

Fig. 3 SEM images of HVOF sprayed WC-10Co-4Cr coating (a,b) and stainless steel

MA

1Cr18Ni9Ti (c,d) after eroded for 10 h at 18 m·s-1 in 3.5 wt.% NaCl slurry (sand content: 10 kg·m-3, sand size: 75~150 mesh)

D

Fig. 4 Nyquist (a,c) plots and Bode plots (b,d) of HVOF sprayed WC-10Co-4Cr

PT E

coating (a,b) and stainless steel 1Cr18Ni9Ti (c,d) in seawater with SRB for different time

CE

Fig. 5 Equivalent circuits used to fit EIS data of HVOF sprayed WC-10Co-4Cr

AC

coating (a,b) and stainless steel 1Cr18Ni9Ti (c,d) in seawater with SRB Fig. 6 Time dependence of Rct of HVOF sprayed WC-10Co-4Cr coating and stainless steel 1Cr18Ni9Ti in seawater with SRB Fig. 7 Potentiodynamic polarization curves of HVOF sprayed WC-10Co-4Cr coating (a) and stainless steel 1Cr18Ni9Ti (b) in seawater with SRB for different time

24

ACCEPTED MANUSCRIPT Tables:

Table 1 Corrosion current densities (icorr) and potentials (Ecorr) values obtained from the potentiodynamic polarization curves of WC-10Co-4Cr coating and stainless steel

PT

1Cr18Ni9Ti in seawater with SRB for different time. icorr (μA·cm-2)

RI

Ecorr (mV) Time

3h

-313

-339

2d

-552

-680

5d

-606

-704

8d

-703

15 d

-610

WC-10Co-4Cr

SC

1Cr18Ni9Ti

1.158

NU

WC-10Co-4Cr

1Cr18Ni9Ti 2.195 1.862

2.171

0.629

-612

1.342

0.713

-716

1.616

1.059

AC

CE

PT E

D

MA

1.359

25

ACCEPTED MANUSCRIPT Highlights  WC-10Co-4Cr coatings were prepared by HVOF spraying.  The coating exhibited higher erosion-corrosion resistance than the stainless steel.  Slurry erosion mechanisms with the augment of NaCl concentration were studied.

PT

 The coating had a comparable microbial corrosion resistance in seawater with

AC

CE

PT E

D

MA

NU

SC

RI

SRB.

26

Figure 1

Figure 2

Figure 3

Figure 4

Figure 5

Figure 6

Figure 7